Electrode assembly, method for manufacturing same, and lithium secondary battery including same
By performing multiple rolling pressures on the positive electrode active material layer of the lithium secondary battery, and using flame retardant electrolyte, the problem of short circuit and fire risk in the charging state of lithium secondary battery is solved, and high energy density is achieved and improve security.
Patent Information
- Application Number
- CN202380035336.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2023-05-31
- Publication Date
- 2024-11-29
AI Technical Summary
In the charging state, the existing lithium secondary batteries cause the positive electrode and the negative electrode to be short-circuited due to the shrinkage of the separator, which increases the risk of ignition, and are easily damaged during the formation of the porous coating, making it difficult to achieve appropriate porosity and mechanical properties.
By performing multiple rolling pressure on the positive electrode active material layer, a porous coating containing polymer binder and zeta potential polymer or ceramic particles is formed, and the porosity is controlled between 20% and 30%, suppressing the coating process. damage and use of flame retardant electrolytes containing flame retardant solvents to improve battery safety.
A stable porous coating is formed in a lithium secondary battery, which improves the electrical insulation between electrodes and the movement ability of lithium ions, reduces the risk of short circuit and fire, and improves the energy density and safety of the battery.
Smart Images

Figure CN119054125A_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0067846 filed in the Korean Intellectual Property Office on June 2, 2022, and Korean Patent Application No. 10-2023-0069510 filed in the Korean Intellectual Property Office on May 30, 2023, the disclosures of which are incorporated herein by reference in their entirety.
[0003] The present invention relates to an electrode assembly, a method for manufacturing the electrode assembly, and a lithium secondary battery comprising the electrode assembly. Background Art
[0004] In recent years, as the application fields of lithium secondary batteries have rapidly expanded to power storage supply for large equipment such as automobiles and power storage devices, and power supply for electronic equipment such as electricity, electronics, communications and computers, the demand for lithium secondary batteries with high capacity, high output, long life and high stability has continued to increase.
[0005] Lithium secondary batteries are generally configured to include a positive electrode, a negative electrode, a separator and an electrolyte, and it is known in the relevant technical field to include a positive electrode that can generate oxygen in a charged state due to an unstable structure. Since the risk of fire when generating oxygen in this way is great, attempts have been made to study and develop methods for enhancing the safety of lithium secondary batteries.
[0006] As an example, a typical separator (e.g., a polyolefin-based porous separator) included in an existing lithium secondary battery may shrink under high temperature conditions, and a short circuit between the positive electrode and the negative electrode may occur due to the shrinkage of the separator. When such a short circuit occurs, it may interact with oxygen generated by the unstable positive electrode, further increasing the risk of fire.
[0007] In order to reduce the risk of fire and improve the safety of lithium secondary batteries, lithium secondary batteries including a porous coating inserted between the positive electrode and the negative electrode to replace or assist the separator can be considered. Such a porous coating can electrically insulate the positive electrode and the negative electrode from each other while enabling ions to move between the positive electrode and the negative electrode.
[0008] However, in the process of forming a coating on the positive electrode or negative electrode, the medium of the composition for forming the coating impregnates the positive electrode, which may cause the problem of swelling of the electrode active material layer. In addition, due to the additional formation of the coating, it is difficult to achieve a proper porosity of the positive electrode active material layer, or problems such as breakage of the active material layer may also occur in the process of forming the coating.
[0009] In view of these problems, there continues to be a need to develop a technology that can satisfactorily form a porous coating on an electrode to replace or assist a separator, thereby solving problems in the process of forming the coating while improving the safety of a secondary battery. Summary of the invention
[0010] [Technical issues]
[0011] The object of the present invention is to provide an electrode assembly and a method for manufacturing the same, which can form a good porous coating on the positive electrode active material layer to improve the safety of the secondary battery and also suppress problems such as damage to the positive electrode active material layer during the formation of the porous coating.
[0012] Another object of the present invention is to provide a lithium secondary battery with improved safety, which includes the above-mentioned electrode assembly.
[0013] [Technical solution]
[0014] According to one embodiment of the present invention, a method for manufacturing an electrode assembly is provided, the method comprising the following steps: (S1) applying a positive electrode slurry to a positive electrode collector and drying it to form a positive electrode active material layer, (S2) rolling the positive electrode collector and the positive electrode active material layer once, (S3) applying a coating slurry to the positive electrode active material layer and drying it to form a positive electrode stack including a coating, (S4) rolling the positive electrode stack a second time, and (S5) stacking a negative electrode on the coating to manufacture an electrode assembly, wherein the first rolling step is performed so that the porosity of the positive electrode active material layer is 35% to 45%, and the second rolling step is performed so that the porosity of the positive electrode active material layer is 20% to 30%.
[0015] According to another embodiment of the present invention, an electrode assembly is provided, which includes: a positive electrode collector, a positive electrode active material layer arranged on the positive electrode collector, a coating coated on the positive electrode active material layer, a mixed layer in which the positive electrode active material layer and the coating are mixed, and a negative electrode arranged on the coating and including a negative electrode collector and a negative electrode active material layer, wherein the coating and the mixed layer contain a polymer binder, and polymer particles or ceramic particles having an absolute value of a zeta potential of 25 mV or more dispersed on the polymer binder, and the thickness of the mixed layer is less than 15 μm.
[0016] According to another embodiment of the present invention, a lithium secondary battery is provided, comprising: a battery case, a flame retardant electrolyte containing a flame retardant solvent having a flash point of 100° C. or above or having no flash point and a lithium salt, and the electrode assembly described above.
[0017] [Beneficial Effects]
[0018] According to the present invention, while optimizing the step of forming a porous coating on the positive electrode active material layer to suppress damage to the positive electrode during the coating formation process, a porous coating that replaces or assists the existing separator can be satisfactorily formed on the positive electrode active material layer, thereby achieving appropriate porosity and mechanical properties of the positive electrode active material layer and the porous coating.
[0019] Therefore, it can greatly contribute to the development of a lithium secondary battery having high capacity characteristics, high energy density, and the like while exhibiting improved safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a photograph of a cross section of the positive electrode active material layer and the coating layer of Example 1 observed by a scanning electron microscope (SEM).
[0021] Figure 2 is a photograph of a cross section of the positive electrode active material layer and the coating layer of Comparative Example 4 observed by a scanning electron microscope (SEM). DETAILED DESCRIPTION
[0022] Hereinafter, the terms or words used in the present specification and claims should not be construed as limited to common or dictionary terms, but the present invention should be interpreted in the meaning and concept consistent with the technical idea of the present invention based on the principle that inventors can appropriately define the concepts of the terms to appropriately describe their own inventions in the best manner.
[0023] Unless otherwise defined, all terms (including technical and scientific terms) used in this specification may be used as the meanings that are generally understood by those of ordinary skill in the art to which the present invention belongs. In addition, unless specifically clearly defined, terms defined in commonly used dictionaries will not be ideally or excessively interpreted.
[0024] The terms used herein are provided to describe embodiments rather than to limit the inventive concept. In this specification, the singular includes the plural, unless the context clearly indicates otherwise. The terms "include" and / or "comprising" used herein do not exclude the presence or addition of one or more elements other than those mentioned.
[0025] Throughout the specification, unless explicitly described to the contrary, the word “comprise” and variations such as “comprises” or “comprising”, will be understood to imply the inclusion of stated elements but not the exclusion of any other elements.
[0026] The term "and / or" used herein, such as in phrases such as "A and / or B", is intended to include "A" (alone), or "B" (alone), or "both A and B".
[0027] Method for manufacturing electrode assembly
[0028] A method for manufacturing an electrode assembly according to one embodiment of the present invention includes the following steps: (S1) applying a positive electrode slurry to a positive electrode collector and drying it to form a positive electrode active material layer; (S2) rolling the positive electrode collector and the positive electrode active material layer once; (S3) applying a coating slurry to the positive electrode active material layer and drying it to form a positive electrode stack including a coating; (S4) rolling the positive electrode stack a second time; and (S5) stacking a negative electrode on the coating to manufacture an electrode assembly, wherein the first rolling step is performed so that the porosity of the positive electrode active material layer is 35% to 45%, and the second rolling step is performed so that the porosity of the positive electrode active material layer is 20% to 30%.
[0029] In the method of manufacturing an electrode assembly, the coating slurry includes, for example, a polymer binder and polymer particles or ceramic particles having an absolute value of zeta potential of 25 mV or more dispersed on the polymer binder, thereby allowing lithium ions to move during charge and discharge while electrically insulating the positive and negative electrodes.
[0030] In the manufacturing method of one embodiment, when a porous coating layer that replaces or assists an existing separator is formed in this way, the positive electrode active material layer and the porous coating layer are formed by multiple rolling steps. It is confirmed that, through this process, a mixed layer can be formed with a very thin thickness, in which a part of the porous coating layer penetrates and mixes into the positive electrode active material layer.
[0031] By forming such a thin porous coating layer, short circuit or ignition between electrodes due to heat shrinkage of the separator can be suppressed, and since the thickness of the porous coating layer is thin, the energy density of the unit secondary battery can be further increased.
[0032] In addition, while finally achieving a porosity suitable for the positive electrode active material layer (e.g., a porosity of 20% to 30%) by performing a plurality of rolling steps, damage to the positive electrode active material layer due to a higher pressure of the rolling step for forming the coating layer, etc. can be suppressed. In addition, due to the plurality of rolling steps, the problem of swelling of the positive electrode active material layer by the liquid medium of the coating slurry can also be reduced.
[0033] On the other hand, each configuration of the electrode assembly will be described in detail below in the description section of the electrode assembly, and each step of the manufacturing method will be described below.
[0034] First, a positive electrode slurry is coated on a positive electrode collector and dried to form a positive electrode active material layer ( S1 ).
[0035] The positive electrode slurry may be prepared by dissolving or dispersing a positive electrode active material, a binder, a conductive material, and optionally a dispersant in a solvent.
[0036] This positive electrode slurry can be applied to the positive electrode current collector and dried to form a positive electrode active material layer. For example, the positive electrode slurry is applied to the positive electrode current collector and passed through a drying area equipped with an exhaust fan at a constant speed in a continuous process, thereby drying the positive electrode current collector and the positive electrode slurry. The drying area can be divided into six areas with a length of about 2m, and the temperature of each drying area can be about 50°C to 95°C.
[0037] Then, the positive electrode current collector and the positive electrode active material layer are subjected to a roll pressing process ( S2 ).
[0038] Such a primary rolling step and a secondary rolling step described below may be performed, for example, by using rolling rollers, and the gap between the rolling rollers may be appropriately set to control the thickness and / or porosity of the positive electrode current collector and the positive electrode active material layer.
[0039] Through the one rolling step, the thickness and / or porosity of the positive electrode current collector and the positive electrode active material layer can be changed within an appropriate range.
[0040] After the first rolling, the total thickness of the positive electrode collector and the positive electrode active material layer after the first rolling is 80% to 90%, or 83% to 87% of the total thickness of the positive electrode collector and the positive electrode active material layer before the first rolling.
[0041] When the thickness ratio after one rolling is less than 80% of the initial thickness, the positive current collector and the positive active material layer are over-rolled, which may cause damage, such as swelling of the positive active material layer on the positive current collector. On the contrary, when the thickness ratio after one rolling exceeds 90% of the initial thickness, the positive current collector and the positive active material layer are substantially not rolled, so that in the subsequent steps, the liquid medium of the coating slurry can penetrate into the positive active material layer and swelling may occur.
[0042] In a specific example, in the initial state without rolling once, the total thickness of the positive electrode collector and the positive electrode active material layer can be 150 μm to 200 μm, or 160 μm to 180 μm, and the total thickness of the positive electrode collector and the positive electrode active material layer after rolling once can be 120 μm to 180 μm or 130 μm to 170 μm.
[0043] In addition, the first rolling step may be performed by passing the positive electrode current collector and the positive electrode active material layer between rolling rollers so that the porosity of the positive electrode active material layer is 35% to 45%, or 37% to 43%.
[0044] At this time, the porosity (P, unit: %) of the positive electrode active material layer may be calculated by a method commonly used in the related technical field. Specifically, the porosity may be calculated according to the following Equation 1.
[0045] [Equation 1]
[0046] P=(1-D) / T x 100
[0047] In Equation 1, D is the density of the positive electrode active material layer, and T is the true density of the positive electrode active material in the positive electrode excluding the current collector. The true density refers to the intrinsic density of the positive electrode active material without pores.
[0048] In addition, the density D of the positive electrode active material layer can be calculated according to the following Equation 2.
[0049] [Equation 2]
[0050] D=M / (S x H)
[0051] In Equation 2, M is the mass of the positive electrode active material layer, S is the area of the positive electrode active material layer, and H is the thickness of the positive electrode active material layer.
[0052] When the porosity of the positive electrode active material layer after one rolling is less than 35%, the positive electrode collector and the positive electrode active material layer are over-rolled, which may cause damage, such as swelling of the positive electrode active material layer on the positive electrode collector. On the contrary, when the porosity of the positive electrode active material layer after one rolling exceeds 45%, the positive electrode collector and the positive electrode active material layer are substantially not rolled, so that in the subsequent steps, the liquid medium of the coating slurry may penetrate into the positive electrode active material layer, and swelling may occur. In addition, due to the penetration of the liquid medium contained in the coating slurry, the porosity of the positive electrode active material layer may increase and uneven pores may be formed.
[0053] Then, the coating slurry is applied onto the positive electrode active material layer and dried to form a positive electrode stack including the coating layer ( S3 ).
[0054] The coating slurry may be, for example, a slurry composition including a polymer binder, polymer particles or ceramic particles having an absolute value of zeta potential of 25 mV or more, and a liquid medium, and may be used to form a porous coating layer (including a mixed layer) on a positive electrode active material layer.
[0055] At this time, the zeta potential of polymer particles or ceramic particles is a physical property that reflects the surface polarity of these particles and defines the electrostatic repulsion or dispersibility between particles. The polymer particles or ceramic particles with a large absolute value of the zeta potential can be evenly dispersed on the positive electrode active material layer, thereby showing a satisfactory and uniform coating performance, and a large number of fine and uniform pores that allow lithium ions to pass between these particles can be defined. In addition, due to the particles that meet this zeta potential, the porous coating can show excellent impregnation performance for a flame retardant electrolyte containing a flame retardant solvent. The combination of a porous coating and a flame retardant electrolyte allows lithium secondary batteries to show more excellent safety.
[0056] The zeta potential of the polymer particles or ceramic particles can be measured, for example, by an electrophoretic light scattering method using a dynamic light scattering device. At this time, the zeta potential of the polymer particles or ceramic particles can be measured in a state where the particles are dispersed in water or an alcohol solvent without a separate dispersant. In a specific example, the zeta potential can be measured in a state where the polymer particles or ceramic particles are dispersed in an aqueous solvent at a concentration of 0.1 wt % or less.
[0057] The absolute value of the zeta potential of the polymer particles or ceramic particles may be 25 mV or more, or 35 mV or more, or 45 mV or more, and 100 mV or less, or 90 mV or less, or 80 mV or less. Within this range, satisfactory coating performance of the coating slurry can be achieved, and high impregnation performance of the flame retardant electrolyte can be ensured.
[0058] Specific examples of the polymer particles include at least one selected from the group consisting of polymethyl (meth)acrylate, polystyrene, polyvinyl chloride, polycarbonate, polysulfone, polyethersulfone, polyetherimide, polyphenylsulfone, polyamideimide, polyimide, polybenzimidazole, polyetherketone, polyphthalamide, polybutylene terephthalate, polyethylene terephthalate, and polyphenylene sulfide.
[0059] In addition, specific examples of the ceramic particles include at least one selected from the group consisting of boehmite, aluminum oxide, titanium oxide, iron oxide, silicon oxide, zirconium oxide, cobalt oxide, tin oxide, nickel oxide, zinc oxide, vanadium oxide, and manganese oxide.
[0060] The zeta potential of polymer particles or ceramic particles can be controlled not only by the type of each particle, but also by the particle size or surface properties of these particles. Therefore, in order to achieve the zeta potential of polymer particles or ceramic particles, dispersibility, or appropriate porosity of porous coatings, etc., the particle size of the polymer particles or ceramic particles can be 50nm to 3μm, 50nm to 1.5μm, or 100nm to 1μm.
[0061] In addition, in order to control the surface properties of the polymer particles or ceramic particles and thereby adjust the zeta potential and the like, the polymer particles or ceramic particles may be included in the coating slurry in a state of being surface-treated with oxygen plasma or ion beams.
[0062] On the other hand, in the above-mentioned coating slurry, the polymer binder used herein may be a polymer of the same type as the binder contained in the positive electrode active material layer, and its specific examples may include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, nitrile rubber, styrene-butadiene rubber or fluororubber, and a mixture or copolymer of two or more selected from these polymers may also be used. However, the specific composition of the polymer binder can obviously be determined by those skilled in the art in consideration of the type and characteristics of the polymer particles or ceramic particles and the method for forming the coating, etc.
[0063] In addition, considering the excellent coating performance of the above coating slurry and the excellent dispersibility of the particles, the coating slurry may include the polymer binder and the polymer particles or ceramic particles in a weight ratio of 5:95 to 40:60, 10:90 to 35:65.
[0064] Also, the coating slurry may further include a dispersant, and such a dispersant may include, for example, at least one of hydrogenated nitrile rubber (H-NBR) and tannic acid.
[0065] In addition, the coating slurry also includes a liquid medium for dispersing the above-mentioned components. This medium can include organic solvents such as N-methyl-2-pyrrolidone (NMP) or acetone, or water, and can be appropriately selected considering the types of the above-mentioned polymer particles, ceramic particles or polymer binders, etc.
[0066] The above coating slurry may be applied onto the once rolled positive electrode active material layer and dried to form a porous coating layer on the positive electrode active material layer, and the resulting product may be defined as a positive electrode stack.
[0067] On the other hand, after the porous coating layer is formed, the positive electrode stack is subjected to secondary rolling (S4). This secondary rolling step can be performed by appropriately setting the gap between the rolling rollers in the same manner as the primary rolling step, and the thickness and / or porosity of the positive electrode active material layer and the porous coating layer can be appropriately achieved by the secondary rolling step.
[0068] After the secondary rolling, the total thickness of the secondary rolled positive electrode collector and the positive electrode active material layer may be 60% to 75%, or 63% to 72% of the total thickness of the non-rolled positive electrode collector and the positive electrode active material layer before the primary rolling. At this time, the thickness of the secondary rolled positive electrode active material layer may be calculated by considering the thickness of the mixed layer in which the porous coating layer is mixed, and the thickness of each layer may be confirmed by electron microscope analysis or the like.
[0069] When the thickness ratio after the secondary rolling is less than 60% of the initial thickness, the positive electrode stack is over-rolled, the thickness of the porous coating becomes too thin, so that the positive electrode and the negative electrode are easily short-circuited, or the positive electrode active material layer may be damaged. On the contrary, when the thickness ratio after the secondary rolling exceeds 75% of the initial thickness, the positive electrode active material layer cannot have an appropriate porosity, and the battery characteristics may deteriorate.
[0070] In addition, the second rolling step may be performed by passing the positive electrode stack between rolling rollers so that the porosity of the positive electrode active material layer is 20% to 30%, or 22% to 28%.
[0071] When the porosity of the positive electrode active material layer after the secondary rolling is less than 20%, the positive electrode stack is over-rolled, the thickness of the porous coating becomes too thin, so that the positive electrode and the negative electrode may be easily short-circuited, or the positive electrode active material layer may be damaged. On the contrary, when the porosity of the positive electrode active material layer after the secondary rolling exceeds 30%, the positive electrode active material layer cannot have an appropriate porosity, and the capacity characteristics of the battery may deteriorate.
[0072] Then, a negative electrode is stacked on the porous coating layer to manufacture an electrode assembly ( S5 ).
[0073] As will be described later, the negative electrode may include a negative electrode current collector and a negative electrode active material layer. In addition, in the step of manufacturing the electrode assembly, the negative electrode is stacked on the porous coating layer in a state where the porous coating layer is formed on the upper surface of the secondary rolled positive electrode stack, thereby manufacturing the electrode assembly.
[0074] An embodiment of an electrode assembly that may be manufactured by a method of one embodiment will be described in detail below.
[0075] Electrode assembly
[0076] An electrode assembly of another embodiment of the present invention includes: a positive electrode collector; a positive electrode active material layer arranged on the positive electrode collector; a coating coated on the positive electrode active material layer; a mixed layer in which the positive electrode active material layer and the coating are mixed; and a negative electrode arranged on the coating and including a negative electrode collector and a negative electrode active material layer, wherein the coating and the mixed layer contain a polymer binder and polymer particles or ceramic particles having an absolute value of a zeta potential of 25 mV or more dispersed on the polymer binder, and the thickness of the mixed layer is less than 15 μm.
[0077] The coating layer includes, for example, a plurality of pores having a diameter of 10 nm or more, and may also be formed of a porous coating layer having a porosity comparable to that of the positive electrode active material layer. Such a porous coating layer electrically insulates the positive electrode and the negative electrode, and also enables lithium ions to move during charging and discharging, thereby replacing or assisting the existing separator.
[0078] In the electrode assembly of other embodiments, since such a porous coating is formed, short circuit or ignition between electrodes caused by thermal contraction of the existing separator can be suppressed, and a lithium secondary battery with improved safety can be provided. In addition, since the formation of the mixed layer is minimized, the porous coating can have a smaller thickness, so the energy density of the unit secondary battery can be further improved.
[0079] In the electrode assembly of other embodiments, the thickness of the mixed layer may be 0 μm to 15 μm, or 0.1 μm to 10 μm, or 1 μm to 5 μm, specifically 5 μm to 14 μm, or 7 μm to 12 μm. The thickness of the mixed layer can be adjusted by controlling the degree of the primary rolling.
[0080] Specifically, a rolling process is performed once so that the total thickness of the positive electrode current collector and the positive electrode active material layer after the rolling process is 80% to 90% of the total thickness of the positive electrode current collector and the positive electrode active material layer that are not rolled, thereby achieving the minimum thickness of the above-mentioned mixed layer. In addition, as the porosity of the positive electrode active material layer is 35% to 45% after the rolling process is performed once, the minimum thickness of the above-mentioned mixed layer can be achieved during the secondary rolling process.
[0081] Since the thickness of the mixed layer satisfies the above numerical range, the thickness of the porous coating layer that replaces or assists the separator can be reduced, and the coating performance of the positive electrode active material layer can be improved. In addition, by controlling the thickness of the porous coating layer, the porosity and electrical properties of the positive electrode active material layer can be adjusted within the desired range.
[0082] Meanwhile, since the compositions of the mixed layer and the porous coating layer are the same as those described with respect to the manufacturing method of one embodiment, additional description thereof will be omitted below.
[0083] In addition, in the electrode assembly, the positive electrode current collector is not particularly limited as long as it has conductivity without causing chemical changes in the battery. For example, the current collector may be formed of stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium or silver. This positive electrode current collector may have a thickness of 3 μm to 500 μm, and may have fine protrusions and depressions formed on its surface to enhance the adhesion of the positive electrode active material layer. For example, the positive electrode current collector may be used in various forms, such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabric structures.
[0084] In addition, the positive electrode active material layer on the positive electrode current collector may include a positive electrode active material, and may optionally further include a conductive material, a binder, and the like.
[0085] The positive electrode active material can be a material capable of reversibly inserting and extracting lithium, and the positive electrode active material can particularly include lithium metal oxides containing lithium and at least one metal (such as cobalt, manganese, nickel, or aluminum). More specifically, the lithium metal oxides can include lithium manganese-based oxides (such as, LiMnO2, LiMn2O4, etc.), lithium cobalt-based oxides (such as, LiCoO2, etc.), lithium nickel-based oxides (such as, LiNiO2, etc.), lithium nickel manganese-based oxides (such as, LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2- Z Ni Z O4 (where 0 < Z < 2), etc.), lithium nickel cobalt-based oxides (such as, LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1)), lithium manganese cobalt-based oxides (such as, LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-Z1 Co Z1 O4 (where 0 < Z1 < 2), etc.), lithium nickel manganese cobalt-based oxides (such as, Li(Ni p Co q Mn r )O2 (where 0 < p < 1, 0 < q < 1, 0 < r < 1 and p + q + r = 1) or Li(Ni p1 Co q1 Mn r1 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r1 < 2 and p1 + q1 + r1 = 2), etc.) or lithium nickel cobalt transition metal (M) oxides (such as, Li(Ni p2 Co q2 Mn r2 M s2 )O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r2, and s2 are the atomic fractions of the respective independent elements, where 0 < p2 < 1, 0 < q2 < 1, 0 < r2 < 1, 0 < s2 < 1 and p2 + q2 + r2 + s2 = 1), etc.), and any one of them or two or more of the compounds thereof can be used.
[0086] Among these materials, in terms of improving the capacity characteristics and stability of the battery, the lithium metal oxides can include LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxides (such as, Li(Ni 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co0.2 )O2、Li(Ni 0.5 Mn 0.3 Co 0.2 )O2、Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.) or lithium nickel manganese cobalt aluminum oxide (e.g., Li(Ni 0.86 Co 0.05 Mn 0.07 Al 0.02 )O2) and the like, and any one of them or a mixture of two or more thereof can be used.
[0087] The content of the positive electrode active material may be 60 to 99 wt %, 70 to 99 wt %, or 80 to 98 wt % based on the total weight of the positive electrode active material layer.
[0088] The conductive material is a component that further improves the conductivity of the positive electrode active material. This conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the battery, and for example, conductive materials such as: carbon powder, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black; graphite powder, such as natural graphite, artificial graphite or graphite with a very developed crystal structure; conductive fibers such as carbon fibers or metal fibers; carbon fluoride powder; conductive powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; or polyphenylene derivatives.
[0089] Generally, the content of the conductive material may be 1 to 20 wt %, 1 to 15 wt %, or 1 to 10 wt % based on the total weight of the positive electrode active material layer.
[0090] Meanwhile, the binder is a component that facilitates bonding between the active material and the conductive material and bonding with the positive electrode current collector.
[0091] Examples of the binder may include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, various copolymers, and the like.
[0092] Generally, the binder may be included in an amount of 1 to 20 wt %, 1 to 15 wt %, or 1 to 10 wt % based on the total weight of the positive electrode active material layer.
[0093] Meanwhile, the negative electrode may include a negative electrode current collector and a negative electrode active material layer.
[0094] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with one of carbon, nickel, titanium or silver, or aluminum-cadmium alloy, etc. can be used.
[0095] The negative electrode current collector may generally have a thickness of 3 μm to 500 μm. Moreover, similar to the positive electrode current collector, the negative electrode current collector may have fine protrusions and depressions formed on its surface to enhance the adhesion of the negative electrode active material. For example, the negative electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, and a non-woven fabric structure.
[0096] In addition, the negative electrode active material layer may contain a negative electrode active material, and may optionally further contain a conductive material, a binder, and the like.
[0097] The negative electrode active material may include at least one selected from the group consisting of lithium metal, carbon materials capable of reversibly intercalating / deintercalating lithium ions, metals or alloys of lithium and these metals, metal composite oxides, materials dopable and dedopable with lithium, and transition metal oxides.
[0098] As a carbon material capable of reversibly embedding / de-embedding lithium ions, any carbon material can be used without particular limitation, as long as it is a carbon-based negative electrode active material commonly used in lithium ion secondary batteries, and as a typical example, crystalline carbon, amorphous carbon or both thereof can be used. An example of crystalline carbon can be graphite, such as irregular, planar, flaky, spherical or fibrous natural graphite or artificial graphite, and an example of amorphous carbon can be soft carbon (low temperature calcined carbon) or hard carbon, mesophase pitch carbide and fired coke.
[0099] As the metal or the alloy of lithium and these metals, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn or the alloy of lithium and these metals can be used.
[0100] As the metal composite oxide, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li xFe2O3(0 < x ≤ 1), Li x WO2(0 < x ≤ 1) and Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Groups I, II, and III in the periodic table, or halogens; 0 < x < 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8), one kind in the group.
[0101] The materials that can be doped and de-doped with lithium can include Si, SiO x (0 < x ≤ 2), Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, and Sn-Y (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and a mixture of SiO2 and at least one of them can also be used. The element Y can be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0102] Transition metal oxides can include lithium-containing titanium composite oxides (LTO), vanadium oxides, and lithium vanadium oxides, etc.
[0103] Based on the total weight of the negative electrode active material layer, the content of the negative electrode active material can be 60 to 99 wt%, or 70 to 99 wt%, or 80 to 98 wt%.
[0104] On the other hand, the types of the binder and the conductive material that can be included in the negative electrode active material layer and the contents of these materials are basically the same as those described for the positive electrode active material layer, and the additional description thereof will be omitted below.
[0105] Lithium secondary battery
[0106] According to another embodiment of the present invention, a lithium secondary battery is provided, which includes: a battery case, a flame-retardant electrolyte containing a flame-retardant solvent with a flash point of 100 °C or higher or having no flash point and a lithium salt, and the above electrode assembly.
[0107] This lithium secondary battery includes a flame retardant electrolyte containing a flame retardant solvent and an electrode assembly containing the above-mentioned porous coating. As described above, the porous coating includes polymer particles or ceramic particles with predetermined characteristics, so that excellent impregnation performance for the flame retardant solvent and the electrolyte can be exhibited. Therefore, the combination of the porous coating and the flame retardant electrolyte more effectively suppresses the ignition caused by the short circuit between the electrodes, thereby further improving the safety of the lithium secondary battery and achieving excellent electrical performance.
[0108] This flame retardant solvent is a solvent with low volatility and low flammability, which can be defined by a predetermined flash point. For example, the flame retardant solvent may include an organic solvent that is substantially non-flammable and does not have a flash point and an organic solvent with a high flash point and low volatility of more than 100°C, or 100°C to 250°C, or 110°C to 200°C. The lithium secondary battery includes a flame retardant electrolyte comprising such a flame retardant solvent and a lithium salt, so that excellent safety and stability can be exhibited. In addition, since the flame retardant electrolyte can be uniformly impregnated into the above-mentioned porous coating, the excellent electrochemical characteristics of the lithium secondary battery can be achieved. The flash point of the flame retardant solvent can be measured using a closed tester or an open tester according to the standard method of ASTM D93 or ASTM D1310.
[0109] In a specific example, the flame retardant solvent may be an organic solvent having a functional group selected from the group consisting of functional groups that may contribute to the low volatility and flame retardancy or non-flammability of the organic solvent (e.g., sulfone functional groups, fluorinated functional groups such as fluorocarbon groups, and phosphorus-containing functional groups such as phosphate groups or phosphonate groups, and nitrile functional groups). More specifically, the flame retardant solvent may include at least one organic solvent selected from the group consisting of sulfone compounds, nitrile compounds, phosphoric acid compounds, and fluorinated carbonate compounds.
[0110] Among them, the sulfone compound may include at least one selected from the group consisting of cyclic sulfone compounds or linear sulfone compounds, specifically, the sulfone compound may include at least one selected from the group consisting of cyclopentane sulfone, ethyl methyl sulfone, dibutyl sulfone, ethyl vinyl sulfone, methyl propyl sulfone, ethyl isopropyl sulfone, ethyl isobutyl sulfone, isopropyl isobutyl sulfone, isopropyl sec-butyl sulfone and butyl isobutyl sulfone.
[0111] In addition, the nitrile compound may include at least one selected from the group consisting of malononitrile, succinonitrile, glutaronitrile, adiponitrile, suberonitrile, and sebaconitrile.
[0112] In addition, the phosphoric acid compound may include at least one selected from the group consisting of dimethyl methyl phosphate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, diethyl ethyl phosphate, dimethyl methyl phosphate, dimethyl (2-methoxyethoxy) methyl phosphonate, diethyl (2-methoxyethoxy) methyl phosphonate and triphenyl phosphate.
[0113] In addition, the fluorinated carbonate compound may include at least one selected from the group consisting of bis(2,2,3,3-tetrafluoropropyl)carbonate, methyl-2,2,2-trifluoroethyl carbonate, ethyl-2,2,2-trifluoroethyl carbonate, propyl-2,2,2-trifluoroethyl carbonate, methyl-2,2,2,2',2',2'-hexafluoroisopropyl carbonate, ethyl-2,2,2,2',2',2'-hexafluoroisopropyl carbonate, di-2,2,2-trifluoroethyl carbonate, 2,2,2-trifluoroethyl-N,N-dimethyl carbonate, hexafluoroisopropyl-N,N-dimethyl carbonate, 4-(2,2,3,3-tetrafluoropropoxymethyl)-[1,3]-dioxolane-2-one and bis(2,2,3,3-pentafluoropropyl)carbonate.
[0114] Meanwhile, the lithium salt contained in the flame retardant electrolyte serves as a medium for transferring ions in the lithium secondary battery. The lithium salt may include, for example, Li + as a cation, and may include at least one selected from the group consisting of: F-, Cl-, Br- - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - , B 10 Cl 10 - 、AlCl4 - 、AlO2 - PF6 - CF3SO3 - 、CH3CO2 - , CF3CO2-, AsF6 - 、SbF6 - 、CH3SO3 - 、(CF3CF2SO2)2N - 、(CF3SO2)2N - 、(FSO2)2N - 、BF2C2O4 - , BC4O8 - PF4C2O4 - PF2C4O8 - 、(CF3)2PF4- 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - 、C4F9SO3 - CF3CF2SO3 - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - CF3(CF2)7SO3 - and SCN - .
[0115] Specifically, the lithium salt may include a salt selected from the group consisting of LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (lithium bis(fluorosulfonyl)imide, LiN(SO2F)2), LiBETI (lithium bis(perfluoroethanesulfonyl)imide, LiN(SO2CF2CF3)2 and LiTFSI (lithium bis(trifluoromethanesulfonyl)imide, LiN(SO2CF3)2), but considering the excellent stability, it is preferred to include LiN(SO2CF3)2. In addition, lithium salts commonly used in electrolytes for lithium secondary batteries can be used without particular limitation.
[0116] The concentration of the lithium salt can be appropriately changed within a generally available range, but in order to obtain the best effect of forming a corrosion prevention film on the electrode surface, the lithium salt can be contained in the flame retardant electrolyte at a concentration of 0.5 M to 6 M, 1 M to 3 M, or 1 M to 2.5 M. When the concentration of the lithium salt satisfies the above range, the effect of improving the cycle characteristics of the lithium secondary battery during high temperature storage is sufficient, and the viscosity of the flame retardant electrolyte is appropriate, so that the impregnation performance of the flame retardant electrolyte can be improved.
[0117] In addition, the flame-retardant electrolyte can prevent the electrolyte from decomposing in a high-power environment and causing the negative electrode to collapse, or can optionally further contain electrolyte additives in consideration of low-temperature high-rate discharge characteristics, high-temperature stability, and the effect of preventing overcharge or suppressing battery expansion at high temperatures.
[0118] Representative examples of such electrolyte additives include at least one selected from the group consisting of cyclic carbonate compounds, halogenated carbonate compounds, sultone compounds, sulfate compounds, phosphate compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds and lithium salt compounds.
[0119] Among them, cyclic carbonate compounds can include vinylene carbonate (VC) or vinyl ethylene carbonate. Moreover, halogenated carbonate compounds can include fluoroethylene carbonate (FEC). In addition, sultone compounds can include at least one selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethane sultone, 1,3-propylene sultone (PRS), 1,4-butene sultone and 1-methyl-1,3-propylene sultone. Sulfate ester / salt compounds can include vinyl sulfate (Esa), trimethylene sulfate (TMS) or methyl trimethylene sulfate (MTMS), and phosphate ester / salt compounds can include at least one selected from the group consisting of difluorobis(oxalate) lithium phosphate, difluoro lithium phosphate, tetramethyl trimethyl silyl phosphate and tris(2,2,2-trifluoroethyl) phosphate.
[0120] The borate / salt compound may include tetraphenylborate, lithium oxalyldifluoroborate (LiODFB) or lithium bis(oxalate)borate (LiB(C2O4)2, LiBOB), and the nitrile compound may include at least one selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanecarbonitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile and 4-fluorophenylacetonitrile. In addition, the benzene compound may include fluorobenzene, the amine compound may include triethanolamine or ethylenediamine, etc., and the silane compound may include tetravinylsilane. In addition, the lithium salt compound is a compound different from the lithium salt contained in the flame retardant electrolyte, wherein the lithium salt compound may include lithium nitrate, lithium difluorophosphate (LiDFP), LiPO2F2 or LiBF4, etc.
[0121] The electrolyte additive may be included in an amount of 0.1 to 10 wt %, or 0.2 to 8 wt %, or 0.5 to 8 wt %, based on the total weight of the flame-retardant electrolyte, thereby contributing to improving ion conductivity or cycle characteristics.
[0122] The above-mentioned lithium secondary battery can be formed by accommodating the electrode assembly in a shell and injecting and impregnating the flame retardant electrolyte therein, and depending on the shape of the shell, the lithium secondary battery can be a cylindrical, prismatic, pouch or coin-shaped battery. At this time, the battery shell can be a battery shell commonly used in the art, and there is no restriction on the shape according to the battery use. For example, the battery shell can be cylindrical, prismatic, pouch and coin-shaped, etc., but is not limited thereto.
[0123] The above-mentioned lithium secondary battery can be manufactured by inserting the electrode assembly into a suitable battery case and then injecting a flame retardant electrolyte therein. Alternatively, the lithium secondary battery can also be manufactured by the following process: stacking the electrode assembly, then impregnating it with a flame retardant electrolyte, placing the resulting product in a battery case and sealing the case.
[0124] The lithium secondary battery can be used not only as a battery cell used as a power source for small devices, but also preferably as a unit battery of a medium or large battery module including a plurality of battery cells. Preferred examples of medium or large devices include electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and energy storage systems (ESS).
[0125] Hereinafter, the present invention will be described in more detail with reference to specific examples. However, the following examples are only used to help understand the present invention and are not intended to limit the scope of the present invention.
[0126] <Examples and Comparative Examples>
[0127] First, in the following examples, the zeta potential of polymer particles or ceramic particles is measured by an electrophoretic light scattering method using a dynamic light scattering device (product name: ELS-Z) in a state where the polymer particles or ceramic particles are dispersed in an aqueous solvent at a concentration of 0.1 wt % or less at a temperature of 25° C.
[0128] Example 1
[0129] S1: Use Li(Ni 0.8 Mn 0.1 Co 0.1 )O2 was used as a positive electrode active material, and a positive electrode slurry containing such a positive electrode active material was applied to an aluminum current collector and dried to form a positive electrode active material layer. The sum of the thickness of the current collector and the thickness of the positive electrode active material layer was 176 μm.
[0130] S2: Rolling is performed once using a pilot rolling machine so that the sum of the thickness of the current collector and the thickness of the positive electrode active material layer is 150 μm, and the porosity of the positive electrode active material layer is 40%. At this time, the porosity of the positive electrode active material layer is calculated from the true density of the positive electrode active material and the mass, area and thickness of the positive electrode active material layer according to equations 1 and 2.
[0131] S3: coating the coating slurry onto the primary roll-pressed positive electrode active material layer.
[0132] Polymethyl methacrylate (PMMA) polymer particles with a zeta potential of -50 mV and a particle size of 1 μm were placed and dispersed in an N-methyl-2-pyrrolidone (NMP) solvent so that the mass ratio of PMMA: hydrogenated nitrile rubber (H-NBR): polyvinylidene fluoride (PVDF) was 7:1:2, thereby preparing a coating slurry (solid content: 21 wt%).
[0133] The coating slurry is dried to form a positive electrode stack including the coating layer.
[0134] S4: The positive electrode stack is rolled twice using a guide roller press, and the second rolling is performed so that the porosity of the positive electrode active material layer is 26%, and after the second rolling, the sum of the thickness of the positive electrode current collector and the thickness of the positive electrode active material layer is 125 μm.
[0135] S5: stacking a negative electrode on the coating layer to manufacture an electrode assembly.
[0136] As the negative electrode, one containing a copper current collector and graphite as a negative electrode active material was used.
[0137] Comparative Example 1
[0138] S1: The same method as in Example 1 was used.
[0139] S2: The same method as Example 1 was performed except that one roll pressing was performed so that the porosity of the positive electrode active material layer was 26% and the sum of the thickness of the current collector and the thickness of the positive electrode active material layer after the one roll pressing was 125 μm.
[0140] S3: The same method as in Example 1 was used.
[0141] S4: No secondary rolling is performed.
[0142] S5: Performed in the same manner as in Example 1.
[0143] Comparative Example 2
[0144] S1: The same method as in Example 1 was used.
[0145] S2: The same method as Example 1 was performed except that one roll pressing was performed so that the porosity of the positive electrode active material layer was 30% and the sum of the thickness of the current collector and the thickness of the positive electrode active material layer after the one roll pressing was 132 μm.
[0146] S3: The same method as in Example 1 was used.
[0147] S4: The same method as Example 1 was performed except that a second rolling was performed so that the porosity of the positive electrode active material layer was 26% and the sum of the thickness of the positive electrode current collector and the thickness of the positive electrode active material layer after the first rolling was 125 μm.
[0148] S5: Performed in the same manner as in Example 1.
[0149] Comparative Example 3
[0150] S1: The same method as in Example 1 was used.
[0151] S2: The same method as Example 1 was performed except that one roll pressing was performed so that the porosity of the positive electrode active material layer was 48% and the sum of the thickness of the current collector and the thickness of the positive electrode active material layer after the one roll pressing was 173 μm.
[0152] S3: The same method as in Example 1 was used.
[0153] S4: The same method as Example 1 was performed except that a second rolling was performed so that the porosity of the positive electrode active material layer was 26% and the sum of the thickness of the positive electrode current collector and the thickness of the positive electrode active material layer after the first rolling was 125 μm.
[0154] S5: Performed in the same manner as in Example 1.
[0155] Comparative Example 4
[0156] S1: The same method as in Example 1 was used.
[0157] S2: No rolling is performed.
[0158] S3: The same method as in Example 1 was used.
[0159] S4: The same method as Example 1 was performed except that a second rolling was performed so that the porosity of the positive electrode active material layer was 26% and the sum of the thickness of the positive electrode current collector and the thickness of the positive electrode active material layer after the second rolling was 125 μm.
[0160] S5: Performed in the same manner as in Example 1.
[0161] <Experimental Example 1>
[0162] Check whether the electrode assembly is damaged
[0163] Whether the electrode assemblies manufactured in Example 1 and Comparative Examples 1 to 4 were damaged was visually confirmed and judged as follows. The measurement results are shown in Table 1 below.
[0164] In order to confirm whether the electrode assembly is damaged, after one rolling in step (S2), visually judge whether swelling occurs at the boundary between the area of the electrode assembly where the positive electrode active material layer is formed and the collector area where the positive electrode active material layer is not formed. If swelling occurs, the electrode assembly is judged to be damaged.
[0165] In addition, it was visually judged whether cracks occurred on the coating surface, and if cracks occurred, it was judged that the electrode assembly was damaged.
[0166] O: Swelling was observed on the current collector, or cracks were observed on the coating surface.
[0167] X: No swelling was observed on the current collector, and no cracks were observed on the coating surface.
[0168] [Table 1]
[0169] Is the electrode assembly damaged? Example 1 X Comparative Example 1 O Comparative Example 2 O Comparative Example 3 O Comparative Example 4 O
[0170] In the case of Example 1, after one roll pressing in step (S2), swelling did not occur at the boundary between the region where the positive electrode active material layer was formed and the current collector region where the positive electrode active material layer was not formed, and no cracks were found in the coating layer.
[0171] In the case of Comparative Examples 1 and 2, swelling occurred at the boundary between the region where the positive electrode active material layer was formed and the current collector region where the positive electrode active material layer was not formed after the one-time rolling in step (S2).
[0172] In the case of Comparative Example 3, no swelling was observed in step (S2), but in step (S3), when the coating slurry was applied to the once rolled positive electrode active material layer, the organic solvent of the coating slurry penetrated into the positive electrode active material layer. As a result, the positive electrode active material layer was easily separated from the electrode assembly, and cracks were observed on the surface of the dried coating.
[0173] In the case of Comparative Example 4, no swelling was observed in step (S2), but when the coating slurry was applied to the positive electrode active material layer in step (S3), the organic solvent of the coating slurry penetrated into the positive electrode active material layer. As a result, the positive electrode active material layer was easily detached from the electrode assembly, and cracks were found on the surface of the dried coating.
[0174] <Experimental Example 2>
[0175] Confirm the thickness of the mixed layer of the electrode assembly
[0176] For Example 1 and Comparative Example 4, the thickness of the mixed layer was confirmed by taking a photograph of a cross section of each positive electrode and the coating layer using a scanning electron microscope (SEM).
[0177] The thickness of the mixed layer is defined as the maximum depth of the coating layer that penetrates into the positive electrode active material layer from the boundary point between the positive electrode active material layer and the coating layer in a photograph of the cross section of the positive electrode and the coating layer.
[0178] The SEM images of Example 1 and Comparative Example 4 are shown in Figure 1 and 2 The measured thicknesses of the mixed layers of Example 1 and Comparative Example 4 are shown in Table 2 below.
[0179] [Table 2]
[0180] Thickness of mixed layer (unit: μm) Example 1 ~0.1 Comparative Example 4 15
[0181] In Example 1, unlike Comparative Example 4, roll pressing was performed once so that the positive electrode active material layer had appropriate porosity, and it was confirmed that in Example 1, the mixed layer in which the positive electrode active material layer and the coating layer were mixed existed only in a very thin thickness.
Claims
1. A method for manufacturing an electrode assembly, the method comprising the following steps: (S1) applying a positive electrode slurry onto a positive electrode current collector and drying it to form a positive electrode active material layer; (S2) rolling the positive electrode current collector and the positive electrode active material layer once; (S3) applying the coating slurry onto the positive electrode active material layer and drying it to form a positive electrode stack including the coating; (S4) performing secondary roll pressing on the positive electrode stack; and (S5) stacking a negative electrode on the coating layer to manufacture an electrode assembly, The first rolling step is performed so that the porosity of the positive electrode active material layer is 35% to 45%, and the second rolling step is performed so that the porosity of the positive electrode active material layer is 20% to 30%.
2. The method for manufacturing an electrode assembly according to claim 1, wherein: The coating slurry includes a polymer binder, polymer particles or ceramic particles having an absolute value of zeta potential of 25 mV or more, and a liquid medium.
3. The method for manufacturing an electrode assembly according to claim 2, wherein: The coating slurry contains the polymer binder and the polymer particles or ceramic particles in a weight ratio of 5:95 to 40:
60.
4. The method for manufacturing an electrode assembly according to claim 2, wherein: The particle size of the polymer particles or ceramic particles is 50 nm to 3 μm.
5. The method for manufacturing an electrode assembly according to claim 1, wherein: The total thickness of the positive electrode collector and the positive electrode active material layer after the single rolling is 80% to 90% of the total thickness of the positive electrode collector and the positive electrode active material layer before the single rolling.
6. The method for manufacturing an electrode assembly according to claim 1, wherein: The total thickness of the positive electrode collector and the positive electrode active material layer after the second rolling is 60% to 75% of the total thickness of the positive electrode collector and the positive electrode active material layer before the first rolling.
7. The method for manufacturing an electrode assembly according to claim 2, further comprising: The polymer particles or ceramic particles are plasma treated to adjust the absolute value of the zeta potential to above 25 mV.
8. An electrode assembly comprising: Positive electrode current collector; a positive electrode active material layer disposed on the positive electrode current collector; a coating layer applied on the positive electrode active material layer; a mixed layer in which the positive electrode active material layer and the coating layer are mixed; a negative electrode disposed on the coating layer and comprising a negative electrode current collector and a negative electrode active material layer, The coating layer and the mixed layer include a polymer binder and polymer particles or ceramic particles dispersed on the polymer binder and having an absolute value of zeta potential of 25 mV or more, and the thickness of the mixed layer is less than 15 μm.
9. The electrode assembly according to claim 8, wherein: The thickness of the mixed layer is 5 μm to 14 μm, and the total thickness of the mixed layer and the coating layer is 5 μm to 50 μm.
10. The electrode assembly according to claim 8, wherein: The particle size of the polymer particles or ceramic particles is 50 nm to 3 μm.
11. The electrode assembly according to claim 8, wherein: The coating layer and the mixed layer include the polymer binder and the polymer particles or ceramic particles in a weight ratio of 5:95 to 40:
60.
12. The electrode assembly according to claim 8, wherein: The polymer particles include at least one selected from the group consisting of polymethyl (meth)acrylate, polystyrene, polyvinyl chloride, polycarbonate, polysulfone, polyethersulfone, polyetherimide, polyphenylsulfone, polyamideimide, polyimide, polybenzimidazole, polyetherketone, polyphthalamide, polybutylene terephthalate, polyethylene terephthalate and polyphenylene sulfide.
13. The electrode assembly according to claim 8, wherein: The ceramic particles include at least one selected from the group consisting of boehmite, aluminum oxide, titanium oxide, iron oxide, silicon oxide, zirconium oxide, cobalt oxide, tin oxide, nickel oxide, zinc oxide, vanadium oxide, and manganese oxide.
14. A lithium secondary battery comprising: A battery case, a flame retardant electrolyte containing a flame retardant solvent having a flash point of 100° C. or above or having no flash point and a lithium salt, and an electrode assembly as defined in claim 8.