Secondary aluminum ash harmless treatment method and progress monitoring method and application thereof
By adding appropriate amount of water and composite accelerator to the secondary aluminum ash, and performing partial water addition and continuous grinding, the problem of reducing reaction rate caused by excessive water is solved, the harmless treatment efficiency is improved, and the process is simplified The process and reduce construction costs and are suitable for industrial applications.
Patent Information
- Application Number
- CN202411446698.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing harmless treatment methods of secondary aluminum ash, excessive water volume leads to a decrease in the reaction rate, the process takes a long time, and a single promoter can easily lead to temperature instability, affecting the treatment efficiency.
Under sealing conditions, add 35 to 50% water and 1 to 2% compound accelerator (sodium bicarbonate, calcium hydroxide and silicone quaternary ammonium salt) to the secondary aluminum ash and mix and react. Add water in batches and continue. Grind, control the evaporation of water, avoid agglomeration, and ensure sufficient reaction.
The efficiency of harmless treatment of secondary aluminum ash is improved, drying and wastewater treatment is simplified, construction costs are reduced, and construction is suitable for industrial treatment, ensuring the comprehensive utilization of aluminum ash resources.
Smart Images

Figure BDA0005087917680000051 
Figure BDA0005087917680000091 
Figure BDA0005087917680000092
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary aluminum ash recovery, and specifically relates to a secondary aluminum ash harmless treatment method and a progress monitoring method and application thereof. Background Art
[0002] Aluminum ash is a characteristic solid waste in the aluminum smelting and casting production process. Before the revision of the "National List of Hazardous Wastes", it was usually used as a general industrial solid waste and was widely used as an alternative raw material in the fields of metal aluminum recycling, water purifier production, steelmaking deoxidizer production, cement clinker production, etc. However, since aluminum ash contains aluminum nitride (AlN) and is easily hydrolyzed to produce ammonia (NH3), the "National List of Hazardous Wastes (2021 Edition)" (hereinafter referred to as the "Hazardous Waste List") implemented on January 1, 2021 clearly defined aluminum ash as a reactive hazardous waste, and the management requirements were tightened, resulting in the problem of aluminum ash disposal becoming a bottleneck restricting the development of the aluminum industry.
[0003] As one of the provinces with the most developed aluminum industry in the country, Guangdong Province produces nearly one million tons of aluminum ash each year, but there are serious shortcomings in the utilization and disposal capabilities of related hazardous waste. In response to this, the Provincial Department of Ecology and Environment issued the "Notice on Strengthening the Prevention and Control of Environmental Pollution from Aluminum Ash Slag" (Guangdong Environmental Office Letter
[2021] No. 57) in 2021, requiring all cities and municipalities to scientifically plan and promote the construction of relevant hazardous waste utilization and disposal projects, accelerate the formation of utilization and disposal capabilities, and effectively guarantee the legal and standardized utilization and disposal needs.
[0004] Although aluminum ash is defined as hazardous waste due to its reactivity, its main components, aluminum (Al) and aluminum oxide (Al2O3), are both valuable substances with certain resource attributes, and should be used for comprehensive resource utilization after harmless treatment. The core of harmless treatment of aluminum ash is to eliminate its hazardous properties. The basic principle is to remove reactive substances or destroy the path of chemical reactions, that is, to remove AIN or hinder the hydrolysis reaction of AlN. The mainstream disposal method is to hydrolyze to remove reactive substances, commonly known as wet disposal process, which has been widely used in actual engineering projects.
[0005] For example, the patent document with application number CN202111317619.1 discloses a method for low-temperature harmless wet treatment of aluminum ash, which is carried out according to the following steps: (1) grinding the secondary aluminum ash, and then screening out the part with a particle size of less than 16 mesh, making a powder and mixing it with a leaching agent, heating and stirring to react, and making a reaction slurry; (2) filtering the reaction slurry, washing and drying the filter residue to make a dry material; (3) adding sulfuric acid solution to the dry material, heating and stirring to react, and making a secondary reaction slurry; (4) filtering the secondary reaction slurry to obtain a filtrate as an aluminum sulfate solution.
[0006] The above-mentioned prior art avoids the dangers of flammability and explosion when treating aluminum ash dust on a large scale, improves the safety of operation, and is simple to operate; it is carried out at low temperature, avoiding the dangers brought by high temperature experiments and reducing energy consumption; it can realize the resource utilization of secondary aluminum ash and turn waste into treasure. However, the mass ratio of water to aluminum ash disclosed is 10 to 17:1. Adding excessive water to aluminum ash will absorb heat, thereby reducing the efficiency of the hydrolysis reaction. At the same time, the addition of excessive water leads to the inevitable design of the operation of removing excess water in the recovery process to dry the aluminum ash, resulting in a long recovery process of the overall process.
[0007] In summary, the present invention aims to provide a secondary aluminum ash harmless treatment method with less water consumption and higher recovery and treatment efficiency. Summary of the invention
[0008] In view of the problems in the related technology, the present invention proposes a secondary aluminum ash harmless treatment method and a progress monitoring method and application thereof to overcome the above-mentioned technical problems existing in the existing related technology.
[0009] The technical solution of the present invention is achieved in this way:
[0010] A method for harmless secondary aluminum ash, wherein an accelerator and water are added to the secondary aluminum ash under sealed conditions for mixed reaction, and the highest temperature during the reaction process does not exceed 100°C;
[0011] The amount of water added is 35-50wt% of the secondary aluminum ash, and the water is added to the secondary aluminum ash at least twice;
[0012] The added amount of the accelerator is 1-2wt% of the secondary aluminum ash, and the accelerator includes sodium bicarbonate, calcium hydroxide and organic silicon quaternary ammonium salt.
[0013] First, compared with the prior art, the amount of water added in the present invention is 35-50wt% of the secondary aluminum ash, which can effectively avoid the problem of heat absorption caused by adding excessive water and resulting in a decrease in the reaction rate, and can effectively improve the efficiency of harmless treatment of secondary aluminum ash. At the same time, it also simplifies the subsequent treatment operations and duration such as secondary aluminum ash drying and industrial wastewater disposal, and even no industrial wastewater is generated.
[0014] Secondly, the present invention designs a specific composite accelerator. The inventors found in the research and development process that the use of calcium hydroxide as a single accelerator is prone to agglomeration, which affects the treatment efficiency of the present invention. The use of sodium bicarbonate alone causes the system of the present invention to be too high in temperature, resulting in rapid evaporation of the added, specific proportion of water, which in turn causes insufficient water content in the secondary aluminum ash, which has an adverse effect on the hydrolysis reaction. The specific selection of organosilicon quaternary ammonium salt is because it has good compatibility with the system of the present invention. The components of the composite accelerator have good synergistic effects, thereby improving the harmless treatment efficiency of the secondary aluminum ash of the present invention.
[0015] Thirdly, based on the specific design of the amount of water added in the present invention, the inventors also found that compared with adding water to the secondary aluminum ash all at once, adding water in batches can control and reduce the amount of water evaporation and avoid insufficient water content in the secondary aluminum ash.
[0016] Finally, the present invention simplifies the steps of harmless treatment of secondary aluminum ash, and is easy to scale up the technology to achieve industrial and batch treatment of secondary aluminum ash. Compared with the current domestic unified regulation of centralized utilization and disposal of secondary aluminum ash, the construction cost is lower, and it is especially suitable for medium and large aluminum enterprises to carry out harmless treatment of secondary aluminum ash and preliminary self-inspection on their own.
[0017] The mixing reaction of secondary aluminum ash and water is prone to agglomeration problems. The agglomerated secondary aluminum ash may only have a surface layer of secondary aluminum ash fully reacted, while the secondary aluminum ash inside has not been effectively rendered harmless and needs to be reworked, affecting the treatment efficiency of the secondary aluminum ash. Therefore, preferably, during the reaction process, the secondary aluminum ash is continuously ground to avoid agglomeration problems and ensure full contact between the secondary aluminum ash and water, thereby achieving full harmless treatment of each batch of aluminum ash.
[0018] More preferably, the grinding speed is 75-85 r / min, and the grinding time is at least 30 min. Too fast a grinding speed may cause the temperature of the system of the present invention to rise too fast or the maximum temperature to exceed the preset temperature, which is not conducive to the reaction of the present invention, for example, it may cause the evaporation of water and thus reduce the water content in the secondary aluminum ash, and the temperature of the grinding device may be too high, which may cause the material processing efficiency to decrease.
[0019] Preferably, water is added to the secondary aluminum ash in batches, first more and then less, and the water is added to the secondary aluminum ash in the form of spraying or atomizing to increase the contact area between water and the secondary aluminum ash, which is beneficial to improving the treatment efficiency of the harmless secondary aluminum ash and the removal of aluminum nitride in the present invention.
[0020] Specifically, the secondary aluminum ash is obtained by high-temperature frying, grinding and screening of aluminum ash.
[0021] Preferably, the mass ratio of the sodium bicarbonate, calcium hydroxide and organosilicon quaternary ammonium salt is 1:2-3:0.12-0.24.
[0022] Preferably, the above-mentioned secondary aluminum ash harmless treatment method comprises the following steps:
[0023] (1) The aluminum ash is roasted at high temperature in a roasting machine, then cooled to 25-35°C until the properties of the material are stable, and then placed in a ball mill for preliminary grinding to an average particle size of ≤0.1mm. The aluminum ash is then sieved to separate the aluminum particles on the sieve and the secondary aluminum ash under the sieve;
[0024] (2) Weighing secondary aluminum ash and accelerator according to a preset mass ratio, adding the secondary aluminum ash and accelerator into a grinding reaction device, adding water for the first time, the amount of water added is 30-40wt% of the secondary aluminum ash, sealing the grinding reaction device, setting the grinding speed to 75-85r / min, and the grinding time is at least 25min;
[0025] (3) Add water for the second time, the amount of water added is 5-10wt% of the secondary aluminum ash, the grinding speed is 75-85r / min, the grinding time is at least 10min, and a small amount of sample is taken to measure the aluminum nitride content ≤5%, that is, the harmless treatment of the secondary aluminum ash is completed.
[0026] The inventors also found during the research and development process that based on the harmless treatment process of the present invention, the material after the grinding reaction is in a high-temperature viscous slurry state, and there is still a lot of ammonia gas inside the material. Ensuring the complete release of ammonia gas is beneficial to further reduce the ammonia content in the material. Therefore, the material after grinding should be spread out to dry, and the spreading thickness should be controlled to be ≤5cm. If the spreading thickness is greater than 5cm, the ammonia gas will not be fully released, and the secondary aluminum ash will become dry and hardened due to cooling, which is not conducive to the continued release of ammonia gas inside.
[0027] The present invention also discloses a progress monitoring method of the above-mentioned secondary aluminum ash harmless treatment method, comprising the following steps:
[0028] (A) Before production begins, test the initial temperature inside the grinding reaction device, i.e., room temperature;
[0029] (B) The first temperature test is performed on the inside of the grinding reaction device from 28 to 32 minutes. If the temperature rises to ≥85°C, it indicates that the reaction is proceeding smoothly.
[0030] (C) A second temperature test is performed at 38 to 42 minutes. If the temperature obtained by the test continues to rise relative to the temperature obtained by the first temperature test and does not exceed 100° C., it indicates that the reaction is proceeding smoothly;
[0031] (D) performing a third temperature test at 58 to 62 minutes, the temperature obtained by the test is lower than the temperature obtained by the second temperature test, and the reaction continues;
[0032] (E) The fourth temperature test is conducted at 78-82 minutes:
[0033] If the temperature obtained by the test continues to drop relative to the temperature obtained by the third temperature test, that is, a small amount of sample is taken to measure the aluminum nitride content ≤5%, it indicates that the harmless treatment of the secondary aluminum ash is completed;
[0034] If the temperature obtained by the test is isothermal or rising relative to the temperature obtained by the third temperature test, it indicates that the harmless treatment of the secondary aluminum ash is still in progress. Then, a temperature test will be carried out every 15 to 20 minutes until two consecutive temperature drops are recorded, that is, a small amount of sample is taken to measure the aluminum nitride content ≤5%, and the harmless treatment of the secondary aluminum ash is completed.
[0035] Based on the technical solution of harmless treatment of secondary aluminum ash of the present invention, temperature measurement time nodes are designed to monitor whether the harmless treatment reaction system of secondary aluminum ash of the present invention is started normally, whether the reaction proceeds normally and judge the progress of the reaction.
[0036] In the first stage of the reaction system of the present invention, a large amount of water is added, and the reaction startup time is long. Therefore, it is designed to confirm the progress of the first reaction in 28 to 32 minutes. Then, the second progress confirmation of the reaction system of the present invention is to confirm whether the reaction continues to proceed normally and at the same time confirm the reaction temperature in the high temperature stage (i.e., step C), and monitor whether the temperature in the high temperature stage exceeds 100°C. Therefore, it is designed to measure the temperature again in the 38th to 42nd minute. If it exceeds this time node, the reaction system of the present invention may have entered the subsequent cooling stage, which will cause the operator to misjudge the progress of the reaction. Therefore, the design of the time node is particularly important for the determination of the progress of the reaction of the present invention, which is convenient for enterprises to check whether the harmless treatment of aluminum ash is in place, and then send it for inspection, so as to minimize the number of rework and the cost of inspection.
[0037] On the other hand, the design uses temperature as a progress monitoring indicator, which is simple and easy to understand, and workers on the harmless aluminum ash process line can quickly master it. Enterprises that apply the secondary aluminum ash harmless treatment method of the present invention have almost no training costs for monitoring work.
[0038] The present invention also discloses the application of the above-mentioned secondary aluminum ash harmless treatment method, which is mainly used for harmless treatment of secondary aluminum ash generated in the process of casting non-ferrous metals. The main chemical components of the secondary aluminum ash generated in the process of casting non-ferrous metals are:
[0039] 65~70wt% Al, 5~6wt% Si, 2~3wt% Mg, 2~3wt% Fe, 1~2wt% Cl, 0.5~1wt% Ca, 0.1~0.3wt% Ti, 0.1~0.5wt% F and 0.05~0.15wt% S. DETAILED DESCRIPTION
[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] The present invention takes the secondary aluminum ash produced by a nonferrous metal product enterprise in Foshan as the research object.
[0042] The aluminum ash just out of the furnace of this enterprise is roasted at high temperature by roasting machine balls, cooled to 25-35℃ until the properties of the material are stable, and then placed in a ball mill for preliminary grinding to an average particle size of ≤0.1mm. The aluminum ash after screening is separated into aluminum particles on the sieve and secondary aluminum ash under the sieve. The secondary aluminum ash is used as the material for treatment in the following embodiments and comparative examples.
[0043] The X-ray fluorescence spectrometry (XRF) method was used to conduct quantitative analysis of the composition of secondary aluminum ash produced by non-ferrous metal products. The results are shown in the table below.
[0044]
[0045] Example 1
[0046] (1) A high energy mortar grinder (Powteq, MG 100) was used as the grinding reaction equipment in this example. The internal temperature of the grinder was tested and recorded, i.e., room temperature, 28°C.
[0047] (2) Weigh 5.000 g of secondary aluminum ash and 0.050 g of accelerator and add them into the grinder. Add 0.750 mL of water in a spraying manner. After sealing, start the grinder. Grind and stir at a speed of 85 r / min for 30 min. At the 30th minute, measure the temperature inside the grinder for the first time and record the temperature, which is 87 °C. The reaction system is heated to a temperature ≥85 °C. The aluminum ash hydrolysis exothermic reaction is proceeding smoothly.
[0048] The accelerator is prepared by mixing sodium bicarbonate (NaHCO3), calcium hydroxide [Ca(OH)2] and organic silicon quaternary ammonium salt (RnSiX4-n, CAS: 27668-52-6) in a mass ratio of 1:2:0.12.
[0049] (3) After adding 1.000 mL of water to the high-energy mortar grinder by spraying, the mixture was stirred at a grinding speed of 85 r / min for 10 min. At the 40th minute, the temperature inside the grinder was measured and recorded for the second time, which was 89° C. The temperature obtained by the test continued to rise relative to the temperature obtained by the first temperature test and did not exceed 100° C. The reaction continued.
[0050] (4) Continue stirring at a grinding speed of 85 r / min for 20 min. At the 60th minute, measure the temperature inside the grinder for the third time and record it, which is 88° C. The temperature obtained by the test is lower than the temperature obtained by the second temperature test, and continue the reaction.
[0051] (5) Stirring was continued at a grinding speed of 85 r / min for 20 min. At the 80th minute, the temperature inside the grinder was measured for the fourth time and recorded as 89° C. The temperature obtained by the test was higher than the temperature obtained by the third temperature test, and the reaction continued.
[0052] (6) The mixture was stirred at a grinding speed of 85 r / min for 20 min. At 100 min, the temperature inside the grinder was measured for the fifth time and recorded as 86° C. The temperature obtained by the test was lower than the temperature obtained by the fourth temperature test, and the reaction was continued.
[0053] (7) Continue to run at a speed of 85 r / min for 20 min. At the 120th minute, measure the temperature inside the grinder for the sixth time and record it, which is 77°C. The temperature obtained by the test is lower than the temperature obtained by the fifth temperature test. Two consecutive temperature drops are recorded. Take 0.200 g of sample for aluminum nitride content test, and the aluminum nitride content is measured to be 0.80%. The aluminum nitride content is ≤5%, and the material is discharged.
[0054] (8) Spread the material out for airing, with a thickness of ≤5 cm, to fully release the ammonia in the slurry. This embodiment completes the harmless treatment of secondary aluminum ash.
[0055] Example 2
[0056] (1) A high energy mortar grinder (Powteq, MG 100) was used as the grinding reaction equipment in this example. The internal temperature of the grinder was tested and recorded, i.e., room temperature, 29°C.
[0057] (2) Weigh 5.000 g of secondary aluminum ash and 0.075 g of accelerator and add them into the grinder. Add 1.500 mL of water in a spraying manner. After sealing, start the grinder. Grind and stir at a speed of 80 r / min for 30 min. At the 30th minute, measure the temperature inside the grinder for the first time and record the temperature, which is 95 °C. The reaction system is heated to a temperature ≥85 °C. The aluminum ash hydrolysis exothermic reaction is proceeding smoothly.
[0058] The accelerator is prepared by mixing sodium bicarbonate (NaHCO3), calcium hydroxide [Ca(OH)2] and organic silicon quaternary ammonium salt (RnSiX4-n, CAS: 27668-52-6) in a mass ratio of 1:2:0.15.
[0059] (3) After adding 0.250 mL of water to the high-energy mortar grinder by spraying, the mixture was stirred at a grinding speed of 80 r / min for 10 min. At the 40th minute, the temperature inside the grinder was measured and recorded for the second time, which was 98° C. The temperature obtained by the test continued to rise relative to the temperature obtained by the first temperature test and did not exceed 100° C. The reaction continued.
[0060] (4) Continue stirring at a grinding speed of 80 r / min for 20 min. At the 60th minute, measure the temperature inside the grinder for the third time and record it at 90° C. The temperature obtained by the test is lower than the temperature obtained by the second temperature test, and continue the reaction.
[0061] (5) Continue stirring at a grinding speed of 80 r / min for 20 min. At the 80th minute, measure the temperature inside the grinder for the fourth time and record 88°C. The temperature obtained by the test is lower than the temperature obtained by the third temperature test. Record two consecutive temperature drops. Take 0.200 g of sample for aluminum nitride content test. The aluminum nitride content is measured to be 0.62%. The aluminum nitride content is ≤5%, and the material is discharged.
[0062] (8) Spread the material out for airing, with a thickness of ≤5 cm, to fully release the ammonia in the slurry. This embodiment completes the harmless treatment of secondary aluminum ash.
[0063] Example 3
[0064] (1) A high energy mortar grinder (Powteq, MG 100) was used as the grinding reaction equipment in this example. The internal temperature of the grinder was tested and recorded, i.e., room temperature, 28°C.
[0065] (2) Weigh 5.000 g of secondary aluminum ash and 0.100 g of accelerator and add them into the grinder. Add 2.000 mL of water in a spraying manner. After sealing, start the grinder. Grind and stir at a speed of 75 r / min for 30 min. At the 30th minute, measure the temperature inside the grinder for the first time and record the temperature, which is 92 °C. The reaction system is heated to a temperature ≥85 °C. The aluminum ash hydrolysis exothermic reaction is proceeding smoothly.
[0066] The accelerator is prepared by mixing sodium bicarbonate (NaHCO3), calcium hydroxide [Ca(OH)2] and organosilicon quaternary ammonium salt (RnSiX4-n, CAS: 27668-52-6) in a mass ratio of 1:3:0.24.
[0067] (3) After adding 0.500 mL of water to the high-energy mortar grinder by spraying, the mixture was stirred at a grinding speed of 75 r / min for 10 min. At the 40th minute, the temperature inside the grinder was measured and recorded for the second time, which was 98° C. The temperature obtained by the test continued to rise relative to the temperature obtained by the first temperature test and did not exceed 100° C. The reaction continued.
[0068] (4) Continue stirring at a grinding speed of 75 r / min for 20 min. At the 60th minute, measure the temperature inside the grinder for the third time and record it, which is 89° C. The temperature obtained by the test is lower than the temperature obtained by the second temperature test, and continue the reaction.
[0069] (5) Continue stirring at a grinding speed of 75 r / min for 20 min. At the 80th minute, measure the temperature inside the grinder for the fourth time and record 80°C. The temperature obtained by the test is lower than the temperature obtained by the third temperature test. Record two consecutive temperature drops. Take 0.200 g of sample for aluminum nitride content test. The aluminum nitride content is measured to be 0.49%. The aluminum nitride content is ≤5%, and the material is discharged.
[0070] (8) Spread the material out for airing, with a thickness of ≤5 cm, to fully release the ammonia in the slurry. This embodiment completes the harmless treatment of secondary aluminum ash.
[0071] Comparative Example 1
[0072] (1) A high energy mortar grinder (Powteq, MG 100) was used as the grinding reaction equipment in this example. The internal temperature of the grinder was tested and recorded, i.e., room temperature, 28°C.
[0073] (2) Weigh 5.000 g of secondary aluminum ash and 0.100 g of accelerator and add them into the grinder. Add 1.500 mL of water in a spraying manner. After sealing, start the grinder. Grind and stir at a speed of 80 r / min for 30 min. At the 30th minute, measure the temperature inside the grinder for the first time and record the temperature, which is 75 °C. The reaction system is heated to a temperature of <85 °C, and the aluminum ash hydrolysis exothermic reaction is slow.
[0074] The accelerator is prepared by mixing sodium bicarbonate (NaHCO3), calcium hydroxide [Ca(OH)2] and organic silicon quaternary ammonium salt (RnSiX4-n, CAS: 27668-52-6) in a mass ratio of 1:2:0.15.
[0075] (3) Continue stirring at a grinding speed of 80 r / min for 10 min. At the 40th minute, measure the temperature inside the grinder for the second time and record it, which is 76°C. The temperature obtained by the test continues to rise relative to the temperature obtained by the first temperature test and does not exceed 100°C, and the reaction continues.
[0076] (4) Continue stirring at a grinding speed of 80 r / min for 20 min. At the 60th minute, measure the temperature inside the grinder for the third time and record it, which is 74° C. The temperature obtained by the test is lower than the temperature obtained by the second temperature test, and continue the reaction.
[0077] (5) The stirring was continued at a grinding speed of 80 r / min for 20 min. At the 80th minute, the temperature inside the grinder was measured for the fourth time and recorded as 70°C. The temperature obtained by the test was lower than the temperature obtained by the third temperature test. Two consecutive temperature drops were recorded. 0.200 g of the sample was taken for aluminum nitride content test. The aluminum nitride content was measured to be 7.49%. The aluminum nitride content was greater than 5%, which did not meet the discharge standard.
[0078] The aluminum nitride (AlN) content test of the above Examples 1 to 3 and Comparative Example 1 includes the following steps:
[0079] (a) Take 0.2000 g of secondary aluminum ash each time, add it to a Kjeldahl flask, connect it to a Kjeldahl nitrogen determination apparatus, and inject 10 mL of sodium hydroxide solution;
[0080] (b) steam distillation for 5 to 10 minutes, collecting the distillate in a conical flask filled with 20 mL of a boric acid solution, the boric acid solution concentration being 20 g / L and pre-added with a mixed indicator, the mixed indicator being prepared by dissolving 0.1 g of bromocresol green and 0.02 g of methyl red in 100 mL of anhydrous ethanol;
[0081] (c) Titrate the collected distillate with aminosulfonic acid standard solution. The endpoint of the titration is when the color of the solution changes from green to pink. Record the titration volume.
[0082] (d) Calculate the nitrogen content after deducting the blank experiment according to the following formula;
[0083] w(N)=(V1-V2)×c×0.014 / m×100%
[0084] Where: w(N) is nitrogen content, %;
[0085] V1 is the volume of aminosulfonic acid standard solution consumed by the sample, mL;
[0086] V2 is the volume of aminosulfonic acid standard solution consumed by the reagent blank, mL;
[0087] c is the concentration of aminosulfonic acid standard solution, mg / mL;
[0088] m is the mass of secondary aluminum ash, g.
[0089] (e) Calculate the AlN content in the secondary aluminum ash according to the following formula.
[0090] w(AIN)=2.929×w(N)
[0091] Where: w(AIN) is the aluminum nitride content, %;
[0092] w(N) is the nitrogen content, %.
[0093] The final products of Examples 1 to 3 were submitted for inspection. The "Hazardous Waste Identification Standard - Reactivity Identification" (GB 5085.5) stipulates that the secondary aluminum ash after harmless treatment should not be reactive. The hazardous characteristic tests of Examples 1 to 3 submitted for inspection all passed.
[0094] In order to prove that the technical solution of the present invention effectively reduces the aluminum nitride content in aluminum ash, and also to prove the change trend and corresponding relationship of "temperature-time-aluminum nitride content", the present invention also records the aluminum nitride content of Examples 1 to 3 and Comparative Example 1 at different time points. The results are as follows:
[0095]
[0096]
[0097]
[0098]
[0099] Based on the data of the above embodiments and comparative examples, it can be concluded that the present invention is capable of effectively rendering secondary aluminum ash harmless and effectively reducing the aluminum nitride content in the secondary aluminum ash. The inspection results also prove that it is reliable to use the aluminum nitride content as a preliminary basis for determining that the secondary aluminum ash has been rendered harmless, and it can be used as a self-inspection standard before an enterprise submits it for inspection, thereby avoiding rework and repeated inspections as much as possible and saving inspection costs. At the same time, it also proves that it is reliable to use the time nodes and temperature changes specified in the present invention as a progress monitoring method.
[0100] The experimental results of Comparative Example 1 show that the amount of water added in the present invention should not be less than 30wt% of the secondary aluminum ash, the hydrolysis reaction of the secondary aluminum ash is difficult to maintain, and the removal efficiency of aluminum nitride is greatly reduced.
[0101] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also change and modify the above implementation modes. Therefore, the present invention is not limited to the specific implementation modes disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A method for harmless treatment of secondary aluminum ash, characterized in that: Under sealed conditions, an accelerator and water are added to the secondary aluminum ash for mixed reaction, and the highest temperature during the reaction process does not exceed 100°C; The amount of water added is 35-50wt% of the secondary aluminum ash, and the water is added to the secondary aluminum ash at least twice; The added amount of the accelerator is 1-2wt% of the secondary aluminum ash, and the accelerator includes sodium bicarbonate, calcium hydroxide and organic silicon quaternary ammonium salt.
2. The method for harmless treatment of secondary aluminum ash according to claim 1, characterized in that: Water is added to the secondary aluminum ash in batches, first more and then less, and the water is added to the secondary aluminum ash in the form of spraying or atomizing.
3. The method for harmless treatment of secondary aluminum ash according to claim 1 or 2, characterized in that: The secondary aluminum ash is obtained by high-temperature frying, grinding and screening of aluminum ash.
4. The method for harmless treatment of secondary aluminum ash according to claim 1 or 2, characterized in that: The mass ratio of the sodium bicarbonate, calcium hydroxide and organosilicon quaternary ammonium salt is 1:2-3:0.12-0.
24.
5. The method for harmless treatment of secondary aluminum ash according to claim 1 or 2, characterized in that: During the reaction process, the secondary aluminum ash is continuously ground.
6. The method for harmless treatment of secondary aluminum ash according to claim 5, characterized in that: The grinding speed is 75-85r / min, and the grinding time is at least 30min.
7. The method for harmless treatment of secondary aluminum ash according to claim 6, characterized in that: The steps include: (1) The aluminum ash is roasted at high temperature in a roasting machine, then cooled to 25-35°C, and initially ground in a ball mill to an average particle size of ≤0.1 mm. The aluminum ash is then sieved to separate the aluminum particles on the sieve and the secondary aluminum ash under the sieve; (2) Weighing secondary aluminum ash and accelerator according to a preset mass ratio, adding the secondary aluminum ash and accelerator into a grinding reaction device, adding water for the first time, the amount of water added is 30-40wt% of the secondary aluminum ash, sealing the grinding reaction device, setting the grinding speed to 75-85r / min, and the grinding time is at least 25min; (3) Add water for the second time, the amount of water added is 5-10wt% of the secondary aluminum ash, the grinding speed is 75-85r / min, the grinding time is at least 10min, and a small amount of sample is taken to measure the aluminum nitride content ≤5%, that is, the harmless treatment of the secondary aluminum ash is completed.
8. The method for harmless treatment of secondary aluminum ash according to claim 7, characterized in that: The ground material is spread out to dry, and the thickness is controlled to be ≤5cm.
9. The progress monitoring method of the secondary aluminum ash harmless treatment method according to any one of claims 1 to 8, characterized in that: The following steps are involved: (A) Before production begins, test the initial temperature inside the grinding reaction device, i.e., room temperature; (B) The first temperature test is performed on the inside of the grinding reaction device from 28 to 32 minutes. If the temperature rises to ≥85°C, it indicates that the reaction is proceeding smoothly. (C) A second temperature test is performed at 38 to 42 minutes. If the temperature obtained by the test continues to rise relative to the temperature obtained by the first temperature test and does not exceed 100° C., it indicates that the reaction is proceeding smoothly; (D) performing a third temperature test at 58 to 62 minutes, the temperature obtained by the test is lower than the temperature obtained by the second temperature test, and the reaction continues; (E) The fourth temperature test is conducted at 78-82 minutes: If the temperature obtained by the test continues to drop relative to the temperature obtained by the third temperature test, that is, a small amount of sample is taken to measure the aluminum nitride content ≤5%, it indicates that the harmless treatment of the secondary aluminum ash is completed; If the temperature obtained by the test is isothermal or rising relative to the temperature obtained by the third temperature test, it indicates that the harmless treatment of the secondary aluminum ash is still in progress. Then, a temperature test will be carried out every 15 to 20 minutes until two consecutive temperature drops are recorded, that is, a small amount of sample is taken to measure the aluminum nitride content ≤5%, and the harmless treatment of the secondary aluminum ash is completed.
10. Application of the secondary aluminum ash harmless treatment method according to any one of claims 1 to 8, characterized in that: The invention is used for harmless treatment of secondary aluminum ash produced in the process of casting non-ferrous metals. The main chemical components of the secondary aluminum ash produced in the process of casting non-ferrous metals are: 65-70wt% Al, 5-6wt% Si, 2-3wt% Mg, 2-3wt% Fe, 1-2wt% Cl, 0.5-1wt% Ca, 0.1-0.5wt% F, 0.1-0.3wt% Ti and 0.05-0.15wt% S.
Citation Information
Patent Citations
Formulation and production of growing media from green organic material
CN1137787A
Wet removal process for fluorine ions in secondary aluminum ash
CN115301715A
Hydrolysis treatment method of aluminum ash
CN115921500A
Magnesium slag harmless treatment method and treatment system
CN116871301A
Secondary aluminum ash denitrification treatment equipment and method
CN118595135A