Method for preparing PMMA (Polymethyl Methacrylate) microsphere emulsion, method for coating diaphragm, electrode and lithium battery

Through the preparation of modified PMMA microsphere emulsion, a three-dimensional network cross-linking structure between the core and the shell is formed, which solves the problem of PMMA septum microspheres dissolution or swelling in the electrolyte, improves the mechanical strength and battery performance of the septum, and reduces the Production cost.

CN119060259AInactive Publication Date: 2024-12-03HUNAN GREEN POWER MATERIAL CO LTD +1

Patent Information

Application Number
CN202411567937.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The microspheres in the existing PMMA diaphragms are easily dissolved or swelled after being soaked in the electrolyte, and the mechanical strength is low, resulting in a reduced permeability of the diaphragm and affecting battery performance.

Method used

The modified PMMA microsphere emulsion preparation method is adopted to form a crosslinking structure with different hydrophobicity through the three-dimensional network crosslinking structure between the core and the shell, which enhances the mechanical strength of the microspheres and improves the coating of the diaphragm by wetting agents and adhesives. Adhesion force to the electrode sheet.

Benefits of technology

The modified PMMA microsphere coated diaphragm retains shape at high temperature and pressure, improving the thermal stability and mechanical strength of the diaphragm, enhancing battery performance, and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060259A_ABST
    Figure CN119060259A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium batteries, and particularly relates to a method for preparing PMMA microsphere emulsion, a method for coating a diaphragm, an electrode and a lithium battery, a PMMA microsphere comprises an inner core, a link layer and a shell, the inner core and the shell are connected through the link layer to form a three-dimensional network cross-linked structure, the inner core is a network structure formed by linking a first acrylic monomer and a cross-linked monomer, and the shell is a three-dimensional network cross-linked structure formed by linking a second acrylic monomer and a cross-linked monomer. The shell is a cross-linked network formed by linking a first acrylic monomer, PMMA (polymethyl methacrylate) and a cross-linking monomer; the method comprises the following steps: mixing 0.05-1.5 parts by mass of an initiator, 50.1-100 parts by mass of a monomer mixture, 100-600 parts by mass of water and 0.05-20 parts by mass of a dispersing agent, and homogenizing to obtain an emulsion; introducing nitrogen into the emulsion at a first preset temperature for a preset ventilation duration; the PMMA microsphere emulsion is obtained by adding 10-50 parts of a first acrylic monomer into the PMMA microsphere, stirring and heating to a second preset temperature while introducing nitrogen, and adding 10-50 parts of a second acrylic monomer to carry out polymerization reaction for a preset reaction time, so that the mechanical strength of the PMMA microsphere is improved, and the performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of lithium battery technology, and in particular to a method for preparing a PMMA microsphere emulsion, a diaphragm coating, an electrode and a lithium battery. Background Art

[0002] PMMA has excellent properties such as good chemical stability and easy processing, and is widely used in new energy, advertising, furniture, construction, medical and other fields. In the current new energy field, PMMA (polymethylmethacrylate) diaphragms are gradually replacing PVDF (polyvinylidene difluoride) diaphragms. The microspheres in the existing PMMA diaphragms are amorphous polymers. After being soaked in electrolyte, they usually dissolve or swell severely. In addition, when external pressure is applied, the mechanical strength is relatively low, and the microspheres are easily deformed, which reduces the air permeability of the diaphragm and thus reduces the battery performance.

[0003] The microspheres of the PMMA diaphragm in the prior art have the problem that they are easily dissolved or swelled after being soaked in electrolyte and have low mechanical strength and large deformation, thereby reducing the air permeability of the diaphragm. Summary of the invention

[0004] The embodiments of the present application provide a method for preparing a PMMA microsphere emulsion, a coating membrane, an electrode, and a lithium battery, which aim to solve to a certain extent the problem that the microspheres in the PMMA membrane are easily dissolved or swelled after being immersed in an electrolyte, have low mechanical strength and large deformation, and reduce the air permeability of the membrane.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing a PMMA microsphere emulsion, wherein the PMMA microsphere comprises a core, a linking layer and a shell, wherein the core and the shell are connected via the linking layer to form a three-dimensional network cross-linked structure, wherein the core is a network structure formed by linking a first acrylic monomer and a cross-linking monomer, and the shell is a cross-linked network formed by linking a second acrylic monomer, PMMA and the cross-linking monomer, wherein the linking layer is formed by linking exposed double bonds of monomers of the core or monomers of the shell via covalent bonds, and wherein a first oil-water partition coefficient of the first acrylic monomer is different from a second oil-water partition coefficient of the second acrylic monomer; Methods include: In parts by mass, at a first preset temperature, 0.05 to 1.5 parts of an initiator, 50.1 to 100 parts of a monomer mixture, 100 to 600 parts of water, and 0.05 to 20 parts of a dispersant are mixed and homogenized to obtain an emulsion; Passing nitrogen gas through the emulsion at the first preset temperature for a preset ventilation time; While passing nitrogen, the temperature is raised to a second preset temperature while stirring; Adding 10 to 50 parts of the second acrylic monomer to carry out polymerization reaction for a preset reaction time to obtain a modified PMMA microsphere emulsion; Wherein, the monomer mixture includes methyl methacrylate, the first acrylic monomer, the cross-linking monomer and a functional monomer.

[0006] In the method for preparing PMMA microsphere emulsion in the embodiment of the present application, compared with the prior art, due to the strong and weak hydrophobicity characteristics between acrylic monomers, the first acrylic monomer, the functional monomer and the cross-linking monomer form a polymer core with a network structure with a strong support effect under the action of an initiator, and the second acrylic monomer, methyl methacrylate and the cross-linking monomer form a cross-linked network shell on the surface of the core through a polymerization reaction under the action of a dispersant, and the exposed double bonds of the monomers of the core or the monomers of the shell are linked by covalent bonds to form a linking layer, and the linking layer connects the core and the shell to form a three-dimensional network cross-linked structure. Since the shell also contains methyl methacrylate, the shell has a mechanical The mechanical strength is greater than that of the inner core, and the inner core, the linking layer and the outer shell constitute modified PMMA microspheres, thereby obtaining a modified PMMA microsphere emulsion; after the modified PMMA microspheres of the embodiment of the present application are soaked in electrolyte, the hydrophobicity of the outer shell is different from that of the inner core, and the outer shell blocks the contact between the inner core and the external electrolyte, thereby reducing the dissolution or swelling of the modified PMMA microspheres, and the coated diaphragm has the characteristic of being non-sticky when rolled up; since both the inner core and the outer shell are in a mesh structure with a strong supporting effect, and a three-dimensional network cross-linked structure is formed by the linking of the linking layer, the mechanical strength of the modified PMMA microspheres is further enhanced, so when external pressure (60°C and 3 Mpa pressure) is applied, no deformation occurs, and a good spherical shape is still maintained. The thermal stability and mechanical strength of the modified PMMA microsphere-coated diaphragm prepared by the embodiment of the present application can meet the production and processing requirements of the battery, thereby improving the performance of the battery.

[0007] In a second aspect, the present application provides a method for preparing a coated diaphragm using a modified PMMA microsphere emulsion obtained by the method described in any one of the first aspects, comprising: By weight, 0.2 parts of the wetting agent was added to water and ultrasonically dissolved to obtain a wetting solution; Adding 10 parts of modified PMMA microsphere emulsion and 0.3 parts of binder to the wetting solution, performing ultrasonic mixing, and filtering to obtain modified PMMA microsphere slurry; The modified PMMA microsphere slurry is uniformly coated on at least one side of the polyolefin separator, and a PMMA microsphere coated separator is obtained by drying. The modified PMMA microsphere coating has a thickness of 2 μm to 20 μm, the polyolefin diaphragm has a thickness of 9 μm to 20 μm, and a pore size of 0.01 μm to 0.3 μm; The drying temperature of the drying treatment is 50° C. to 70° C., and the drying time is 5 min to 10 min.

[0008] The modified PMMA microsphere coated diaphragm of the embodiment of the present application adopts the modified PMMA microsphere emulsion described in any one of the first aspects, and increases the adhesion between the modified PMMA microsphere coated diaphragm and the electrode pole piece by adding a wetting agent and a binder. Therefore, while improving the adhesion between the modified PMMA microsphere coated diaphragm and the electrode pole piece, it also meets the production and processing requirements of the battery in terms of thermal stability and mechanical strength, thereby improving the performance of the battery.

[0009] In a third aspect, an embodiment of the present application provides an electrode, the surface of which is covered with a modified PMMA microsphere-coated diaphragm obtained by the preparation method described in the second aspect.

[0010] Since the electrode surface of the electrode of the embodiment of the present application is covered with a modified PMMA microsphere coated diaphragm obtained by any method in the second aspect, the adhesion between the modified PMMA microsphere coated diaphragm and the electrode pole piece is improved, and at the same time, the production and processing requirements of the battery are met in terms of thermal stability and mechanical strength, thereby improving the performance of the battery.

[0011] In a fourth aspect, an embodiment of the present application provides a lithium battery, comprising the electrode as described in the third aspect.

[0012] The lithium battery of the embodiment of the present application adopts the electrode as described in the third aspect, which improves the adhesion between the modified PMMA microsphere-coated diaphragm and the electrode pole piece in the electrode, and also meets the production and processing requirements of the battery in terms of thermal stability and mechanical strength, thereby improving the performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0014] Figure 1 It is a schematic flow chart of a method for preparing PMMA microsphere emulsion provided in one embodiment of the present application; Figure 2 Schematic diagram of the cross-sectional structure of modified PMMA microspheres provided in one embodiment of the present application; Figure 3 It is a schematic flow chart of a method for preparing a coated diaphragm provided in one embodiment of the present application; Figure 4 is a scanning electron microscope schematic diagram of the modified PMMA microsphere coated diaphragm of Preparation Example 5 of the present application before the pressure resistance test; Figure 5 is a scanning electron microscope schematic diagram of the modified PMMA microsphere coated diaphragm of Preparation Example 5 of the present application after the pressure resistance test; Figure 6 is a scanning electron microscope schematic diagram of the modified PMMA microsphere coated diaphragm of Preparation Example 15 of the present application before the pressure resistance test; Figure 7 is a scanning electron microscope schematic diagram of the modified PMMA microsphere coated diaphragm of Preparation Example 15 of the present application after the pressure resistance test; Figure 8 This is a schematic diagram of a scanning electron microscope of the PMMA microsphere-coated diaphragm prepared in Comparative Example 1 of the present application after a pressure resistance test; Fig. 9 It is a schematic diagram of a scanning electron microscope of the PMMA microsphere-coated diaphragm prepared in comparative example 2 of the present application after a pressure resistance test. DETAILED DESCRIPTION

[0015] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0016] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0017] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, a~b (i.e. a and b), a~c, b~c, or a~b~c, where a, b, c can be single or multiple, respectively.

[0018] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. For example, without departing from the scope of the implementation regulations of this application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0019] The terms used in the embodiments of the present application are only for the purpose of describing specific implementation rules, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the implementation rules of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0020] It should be understood that in the various embodiments of the present application, the size of the serial number of each process does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the implementation regulations of this application.

[0021] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0022] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0023] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0024] In the current new energy field, PMMA diaphragms are gradually replacing PVDF in diaphragms. The microspheres in the existing PMMA diaphragms are amorphous polymers. After being soaked in electrolyte, they usually dissolve or swell, and when external pressure is applied, the mechanical strength is relatively low. The microspheres are easily deformed and block the air pores of the diaphragm, reducing the air permeability of the diaphragm and the speed at which ions pass through, seriously affecting battery performance.

[0025] In order to overcome the above technical problems to a certain extent, the PMMA microspheres of the present application include a core, a linking layer and a shell, the core and the shell are connected by the linking layer to form a three-dimensional network cross-linked structure, the core is a network structure formed by linking the first acrylic monomer and the cross-linking monomer, the shell is a cross-linked network formed by linking the second acrylic monomer, PMMA and the cross-linking monomer, the linking layer is formed by linking the exposed double bonds of the monomers of the core or the monomers of the shell through covalent bonds, and the first oil-water partition coefficient of the first acrylic monomer is different from the second oil-water partition coefficient of the second acrylic monomer. Figure 1 As shown, the first aspect of the embodiment of the present application provides a method for preparing a PMMA microsphere emulsion, comprising: S11, in parts by mass, at a first preset temperature, mixing 0.05 to 1.5 parts of an initiator, 50.1 to 100 parts of a monomer mixture, 100 to 600 parts of water, and 0.05 to 20 parts of a dispersant, and homogenizing to obtain an emulsion, wherein the monomer mixture includes methyl methacrylate, a first acrylic monomer, a crosslinking monomer, and a functional monomer; S12, passing nitrogen gas through the emulsion at a first preset temperature for a preset ventilation time; S13, heating to a second preset temperature while stirring while passing nitrogen; S14, adding 10 to 50 parts of a second acrylic monomer to carry out polymerization reaction for a preset reaction time to obtain a modified PMMA microsphere emulsion.

[0026] In the method for preparing PMMA microsphere emulsion in the embodiment of the present application, compared with the PMMA microsphere emulsion in the prior art, due to the strong and weak hydrophobicity characteristics between acrylic monomers, the first acrylic monomer, the functional monomer and the cross-linking monomer form a polymer core with a network structure having a strong supporting effect under the action of an initiator, and the second acrylic monomer, methyl methacrylate and the cross-linking monomer form a cross-linked network shell on the surface of the core through a polymerization reaction under the action of a dispersant, and the exposed double bonds of the monomers of the core or the monomers of the shell are linked by covalent bonds to form a linking layer, and the linking layer connects the core and the shell to form a three-dimensional network cross-linked structure. Since the shell also contains methyl methacrylate, the mechanical strength of the shell is greater than that of the core, and the core, the linking layer and the shell constitute a modified PMMA microsphere (such as Figure 2As shown), a modified PMMA microsphere emulsion is obtained; after the modified PMMA microspheres of the embodiment of the present application are soaked in electrolyte, the hydrophobicity of the shell and the core is different, and the shell blocks the contact between the hydrophobic core and the external electrolyte, which reduces the dissolution or swelling of the modified PMMA microspheres, and the coated diaphragm has the characteristics of rolling and non-stickiness; because the core and the shell are both in a mesh structure with strong support, and a three-dimensional network cross-linked structure is formed by the linking of the linking layer, the mechanical strength of the modified PMMA microspheres is further enhanced, so when the external pressure (60°C and 3 Mpa pressure) is applied, there is no deformation, and the spherical shape is still maintained. The thermal stability and mechanical strength of the modified PMMA microsphere coated diaphragm prepared by the embodiment of the present application can meet the production and processing requirements of the battery, thereby improving the performance of the battery. In addition, the preparation method of the PMMA microsphere emulsion of the embodiment of the present application is simple in process flow, reduces the number of process steps, and does not use organic solvents such as ethanol, and the production process does not require wastewater treatment of organic solvents, thereby reducing production costs.

[0027] In some embodiments, 0.05 to 1.5 parts of an initiator, 50.1 to 100 parts of a monomer mixture, 100 to 600 parts of water, and 0.05 to 20 parts of a dispersant are mixed, and homogenized to obtain an emulsion, comprising: 0.05-1.5 parts by weight of an initiator, 10-60 parts by weight of methyl methacrylate, 30-60 parts by weight of a first acrylic monomer, 0.1-10 parts by weight of a functional monomer, 100-600 parts by weight of water and 0.05-20 parts by weight of a dispersant are mixed, and a first homogenization is performed to obtain a pre-emulsion; 1-30 parts by weight of a cross-linking monomer is added to the pre-emulsion, and a second homogenization is performed to obtain an emulsion.

[0028] In the embodiment of the present application, since the monomer mixture includes methyl methacrylate, a first acrylic monomer, a cross-linking monomer and a functional monomer, the initiator, methyl methacrylate, the first acrylic monomer, the functional monomer, water and the dispersant are first homogenized so that the components are evenly mixed to obtain a pre-emulsion, and then the cross-linking monomer is added and homogenized to obtain an emulsion. Under the action of the initiator, the first acrylic monomer, the functional monomer and the cross-linking monomer form a polymer core with a network structure having a strong supporting effect at a second preset temperature.

[0029] In some embodiments, the stirring speed of the first homogenization is 2500 rpm to 3000 rpm; the stirring speed of the second homogenization is 2000 rpm to 2500 rpm; the stirring speed of heating while stirring is 150 rpm to 250 rpm; the stirring speed of the first homogenization is relatively high, and the components can be homogenized in a shorter time, thereby improving the mixing speed of the components; after the first homogenization, the stirring speed of the second homogenization is lower than the stirring speed of the first homogenization, which allows the cross-linking monomer to mix with the first acrylic monomer and the functional monomer more quickly; the stirring speed used when heating while stirring can make the emulsion temperature rise more evenly, and also facilitates the cross-linking monomer to polymerize with the first acrylic monomer and the functional monomer more quickly in the subsequent steps.

[0030] In some embodiments, the first preset temperature is 18°C ​​to 25°C, and the preset ventilation time is 10 min to 90 min; the stirring speed while stirring and homogenizing while heating is 240 r / min; the stirring speed when heating to the first preset temperature is reduced to 200r / min. Due to the use of the preset ventilation time of the embodiment of the present application, the oxygen in the suspension is removed as much as possible by nitrogen, and the reaction of free radicals with oxygen in the solution is avoided, and the generation of other unnecessary by-products in the subsequent polymerization reaction is avoided, thereby improving the purity of the polymer in the improved PMMA microsphere emulsion, thereby improving the cross-linking monomer, the functional monomer and the first acrylic monomer The polymer forms a microsphere core with a network support structure, and the stirring speed is reduced when the temperature is raised to the first preset temperature, which can avoid the polymer being broken up by an excessively high stirring speed, thereby maintaining the mechanical strength of the microsphere core.

[0031] In some embodiments, the second preset temperature is 60°C to 90°C; the preset reaction time is 6 h to 12 h. The preset temperature and preset reaction time of the embodiments of the present application are used to increase the speed at which the cross-linking monomer, the functional monomer and the first acrylic monomer form a polymer core with a network structure having a strong supporting effect, and also increase the proportion and speed at which the network structure polymer of the cross-linking monomer and the second acrylic monomer forms a network support structure on the surface of the core. At the same time, the appropriate temperature range maintains the stability of the network support structure formed by the network structure polymer of the cross-linking monomer and the second acrylic monomer on the surface of the core.

[0032] In some embodiments, the particle size D50 of the modified PMMA microsphere emulsion is 2 μm to 20 μm, and the particle size D90 is 2 μm to 50 μm. In the embodiments of the present application, since the particle size D50 of the modified PMMA microsphere emulsion is larger than the pore size of the polyolefin diaphragm, the pore size of the polyolefin diaphragm will not be blocked, thereby avoiding the obstruction of lithium ion transmission and improving the performance of the lithium battery.

[0033] It should be noted that the oil-water partition coefficient is the Log P value, which refers to the logarithm of the ratio of the partition coefficients of a substance in n-octanol (oil) and water. The larger the Log P value (i.e., the oil-water partition coefficient), the more lipophilic and hydrophobic the substance is; the smaller the Log P value (i.e., the oil-water partition coefficient), the more hydrophilic and hydrophobic the substance is.

[0034] In some embodiments, the first oil-water partition coefficient of the first acrylic monomer in the inner core is greater than or equal to 2.5, the second oil-water partition coefficient of the second acrylic monomer in the outer shell is less than 2.5, and the third oil-water partition coefficient of the cross-linking monomer is 1.5 to 2.5; in the embodiments of the present application, since the hydrophobicity of the first acrylic monomer in the inner core is stronger than the hydrophobicity of the second acrylic monomer in the outer shell, the second acrylic monomer will cover the first acrylic monomer in the inner core during the polymerization reaction after homogenization, and the hydrophobicity of the cross-linking monomer is closer to that of the second acrylic monomer. Therefore, after cross-linking with the first acrylic monomer in the inner core, more cross-linking reactions occur with the second acrylic monomer to form a linking layer, thereby tightly connecting the inner core and the outer shell together, further increasing the mechanical strength of the modified PMMA microspheres.

[0035] In some embodiments, the first oil-water partition coefficient of the first acrylic monomer is greater than the second oil-water partition coefficient of the second acrylic monomer, the number of carbon atoms of the first acrylic monomer is greater than or equal to 10, and the number of carbon atoms of the second acrylic monomer is greater than or equal to 4; since the second acrylic monomer in the outer shell has weak hydrophobicity and has a certain hydrophilicity, it blocks the contact between the first acrylic monomer in the strongly hydrophobic inner core and the external electrolyte, further reducing the dissolution or swelling of the modified PMMA microspheres and improving the non-stick performance of the coated diaphragm; since the number of carbon atoms of the first acrylic monomer and the second acrylic monomer is relatively large, the first acrylic monomer is a long-chain acrylic monomer, which can form a larger and more complex network cross-linking structure with the cross-linking monomer, further enhancing the mechanical properties of the modified PMMA microspheres.

[0036] In some embodiments, the first acrylic monomer is a combination of one or more of isooctyl acrylate, lauryl methacrylate, cyclohexyl methacrylate, isobornyl acrylate, and epoxy acrylate; And / or, the second acrylic monomer is a combination of one or more of isobutyl acrylate, 2-ethylbutyl acrylate, and glycidyl methacrylate; And / or, the crosslinking monomer is a combination of one or more of ethylene glycol dimethacrylate, ethoxylated trimethylolpropane triacrylate, and divinylbenzene; and / or, the dispersant is a combination of one or more of polyvinyl alcohol, sodium lauryl sulfate, polyacrylate, and polyvinyl pyrrolidone; and / or, the initiator is a combination of one or more of benzoyl peroxide and azobisisobutyronitrile; And / or, the functional monomer is a combination of one or more of styrene and silane coupling agent.

[0037] In the examples of the present application, the types of acrylic monomers, cross-linking monomers, dispersants, initiators and functional monomers are limited, and the corresponding types can be selected according to the actual production situation, which increases the selectivity of raw materials. The limitation of various types ensures the stability of the modified PMMA microsphere emulsion. Among them, the molecular structure of the cross-linking monomer includes more than or equal to 2 unsaturated bonds that can participate in the polymerization reaction.

[0038] Second, as Figure 3 As shown, the embodiment of the present application provides a method for preparing a coated diaphragm using a modified PMMA microsphere emulsion obtained by the method described in any one of the first aspects, comprising: S21, adding 0.2 parts of a wetting agent by mass into water and dissolving it by ultrasonication to obtain a wetting solution.

[0039] S22, adding 10 parts of the modified PMMA microsphere emulsion and 0.3 parts of the binder to the wetting solution, performing ultrasonic mixing, and filtering to obtain a modified PMMA microsphere slurry.

[0040] S23, uniformly coating the modified PMMA microsphere slurry on at least one side of the polyolefin diaphragm, and obtaining a modified PMMA microsphere coated diaphragm through drying.

[0041] The modified PMMA microsphere coated diaphragm of the embodiment of the present application adopts the modified PMMA microsphere emulsion described in any one of the first aspects, and increases the adhesion between the modified PMMA microsphere coated diaphragm and the electrode pole piece by adding a wetting agent and a binder. Therefore, while improving the adhesion between the modified PMMA microsphere coated diaphragm and the electrode pole piece, it also meets the production and processing requirements of the battery in terms of thermal stability and mechanical strength, thereby improving the performance of the battery.

[0042] In some embodiments, the thickness of the modified PMMA microsphere coating is 2 μm to 20 μm, the thickness of the polyolefin separator is 9 μm to 20 μm, and the pore size is 0.01 μm to 0.3 μm; the drying temperature of the drying treatment is 50°C to 70°C, and the drying time is 5min to 10 min. In the embodiment of the present application, since the thickness of the modified PMMA microsphere coating is the D50 radius of a single modified PMMA microsphere, and the D50 radius of the microsphere is greater than the pore size of the polyolefin separator, the transmission efficiency of lithium ions in the lithium battery is improved. The drying process parameters set in the embodiment of the present application can make the modified PMMA microsphere coating have better processing performance and improve the processing efficiency of the electrode.

[0043] In some embodiments, the wetting agent includes: one or more of lauryl alcohol polyoxyethylene ether, polydimethylsiloxane, polyether siloxane, polyoxyethylene ether, polyoxyethylene alkylamine, polyoxyethylene alkylphenol ether, polyoxyethylene fatty alcohol ether, and octylphenol polyoxyethylene ether; the binder includes: one or more of polyurethane, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl acetate, methacrylic acid, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, ethyl acrylic acid, and ethyl acrylate; the types of wetting agent and binder are selected according to the requirements of the coating membrane, thereby increasing the selectivity of the raw materials, and limiting the types to ensure the stability of the modified PMMA microsphere coated membrane.

[0044] In a third aspect, an embodiment of the present application provides an electrode, the surface of which is covered with a modified PMMA microsphere-coated diaphragm obtained by any method in the second aspect.

[0045] Since the electrode surface of the electrode of the embodiment of the present application is covered with a modified PMMA microsphere coated diaphragm obtained by any method in the second aspect, the adhesion between the modified PMMA microsphere coated diaphragm and the electrode pole piece is improved, and at the same time, the production and processing requirements of the battery are met in terms of thermal stability and mechanical strength, thereby improving the performance of the battery.

[0046] In some embodiments, at 60°C and 3Mpa pressure, the bonding force between the modified PMMA microsphere coated diaphragm and the electrode pole piece is 2.5 N / m to 5.0 N / m. In the embodiments of the present application, since the long-chain olefin monomer is used as the main monomer, the viscosity of the network structure polymer is increased, thereby increasing the bonding force between the modified PMMA microsphere coated diaphragm and the electrode pole piece, increasing the difficulty of peeling between the modified PMMA microsphere coated diaphragm and the electrode pole piece, thereby improving the stability of the lithium battery.

[0047] In a fourth aspect, an embodiment of the present application provides a lithium battery, comprising the electrode as described in the third aspect.

[0048] The lithium battery of the embodiment of the present application adopts the electrode as described in the third aspect, which improves the adhesion between the modified PMMA microsphere-coated diaphragm and the electrode pole piece in the electrode, and also meets the production and processing requirements of the battery in terms of thermal stability and mechanical strength, thereby improving the performance of the battery.

[0049] The technical solution of the present application is illustrated below through specific embodiments and comparative examples.

[0050] Example 1 Step 1), 3.5g of methyl methacrylate, 50g of isooctyl acrylate (first acrylic monomer), 5g of styrene (functional monomer) and 10% of ethylene glycol dimethacrylate (cross-linking monomer) relative to the total mass of the monomer mixture are mixed to form a monomer mixture, 1% of the mass of the monomer mixture is dissolved in benzoyl peroxide (initiator) in the monomer mixture, 200g of water and 5g of polyvinyl alcohol (dispersant) are added and mixed, and homogenized for 15min, and the upper suspension is taken to obtain an emulsion; Step 2), the emulsion is transferred to a reactor and nitrogen is passed through the reactor at a first preset temperature of 18°C ​​to 25°C for 30 minutes; Step 3), while nitrogen was passed through, the temperature was raised to 70°C while stirring, and 3.5 g of isobutyl acrylate (the second acrylic monomer) was added to carry out polymerization reaction for a preset reaction time, and the polymerization reaction was carried out for 8 h to obtain a modified PMMA microsphere emulsion 1.

[0051] Example 2: The difference from Example 1 is that the ratio of ethylene glycol dimethacrylate (cross-linking monomer) to the total mass of the monomer mixture is changed to 20%.

[0052] Example 3: The difference from Example 1 is that the content of ethylene glycol dimethacrylate (cross-linking monomer) relative to the total mass of the monomer mixture is changed to 30%.

[0053] Example 4: The difference from Example 1 is that the cross-linking monomer is changed to ethoxylated trimethylolpropane triacrylate, and the proportion relative to the total mass of the monomer mixture is still 10%.

[0054] Example 5: The difference from Example 1 is that the cross-linking monomer is changed to ethoxylated trimethylolpropane triacrylate, and the proportion relative to the total mass of the monomer mixture is changed to 20%.

[0055] Example 6: The difference from Example 1 is that the cross-linking monomer is changed to ethoxylated trimethylolpropane triacrylate, and the proportion relative to the total mass of the monomer mixture is changed to 30%.

[0056] Example 7: The difference from Example 1 is that the cross-linking monomer is changed to a mixed cross-linking monomer of ethylene glycol dimethacrylate and ethoxylated trimethylolpropane triacrylate, and the ratio of the mixed cross-linking monomer to the total mass of the monomer mixture is changed to 5% ethylene glycol dimethacrylate and 15% ethoxylated trimethylolpropane triacrylate.

[0057] Example 8: The difference from Example 1 is that the cross-linking monomer is changed to a mixed cross-linking monomer of ethylene glycol dimethacrylate and ethoxylated trimethylolpropane triacrylate, and the ratio of the mixed cross-linking monomer to the total mass of the monomer mixture is changed to 10% ethylene glycol dimethacrylate and 10% ethoxylated trimethylolpropane triacrylate.

[0058] Example 9: The difference from Example 1 is that the cross-linking monomer is changed to a mixed cross-linking monomer of ethylene glycol dimethacrylate and ethoxylated trimethylolpropane triacrylate, and the ratio of the mixed cross-linking monomer to the total mass of the monomer mixture is changed to 15% ethylene glycol dimethacrylate and 15% ethoxylated trimethylolpropane triacrylate.

[0059] Example 10: The difference from Example 1 is that the cross-linking monomer is changed to a mixed cross-linking monomer of ethylene glycol dimethacrylate and ethoxylated trimethylolpropane triacrylate, and the mixed cross-linking monomer is changed to 10% ethylene glycol dimethacrylate and 5% ethoxylated trimethylolpropane triacrylate relative to the total mass of the monomer mixture.

[0060] Example 11: The difference from Example 1 is that in step 1), the mass of the cross-linking monomer is fixed and the mass ratio of the olefinic monomer is adjusted.

[0061] Step 1), 3.5 g of methyl methacrylate, 20% of isooctyl acrylate (first acrylic monomer) relative to the total mass of the monomer mixture, 5 g of styrene (functional monomer) and 5 g of ethoxylated trimethylolpropane triacrylate (cross-linking monomer) are mixed to form a monomer mixture, 1% of the mass of the monomer mixture is dissolved in benzoyl peroxide (initiator) in the monomer mixture, and then 200 g of water and 5 g of polyvinyl alcohol (dispersant) are added to obtain a mixed solution.

[0062] Example 12: The difference from Example 11 is that the ratio of isooctyl acrylate (the first acrylic monomer) to the total mass of the monomer mixture is changed to 30%.

[0063] Example 13: The difference from Example 11 is that the ratio of isooctyl acrylate (the first acrylic monomer) to the total mass of the monomer mixture is changed to 40%.

[0064] Example 14: The difference from Example 11 is that the ratio of isooctyl acrylate (the first acrylic monomer) to the total mass of the monomer mixture is changed to 50%.

[0065] Example 15: The difference from Example 11 is that the ratio of isooctyl acrylate (the first acrylic monomer) to the total mass of the monomer mixture is changed to 60%.

[0066] Example 16: The difference from Example 11 is that the ratio of isooctyl acrylate (the first acrylic monomer) to the total mass of the monomer mixture is changed to 70%.

[0067] Example 17: The difference from Example 11 is that the ratio of isooctyl acrylate (the first acrylic monomer) to the total mass of the monomer mixture is changed to 80%.

[0068] Example 18: The difference from Example 1 is that in step 1), the mass of the cross-linking monomer is fixed, and the type and mass ratio of the first acrylic monomer are adjusted.

[0069] Step 1), 3.5 g of methyl methacrylate, 40% of hydroxyethyl acrylate relative to the total mass of the monomer mixture, 20% of ethylene glycol dimethacrylate (cross-linking monomer) relative to the total mass of the monomer mixture, and 5 g of styrene (functional monomer) are mixed to form a monomer mixture, 1% of benzoyl peroxide (initiator) equivalent to the mass of the monomer mixture is dissolved in the monomer mixture, and then 200 g of water and 5 g of polyvinyl alcohol (dispersant) are added to obtain a mixed solution.

[0070] Example 19: The difference from Example 18 is that the first acrylic monomer is changed to epoxy acrylate, and the change relative to the total mass of the monomer mixture is 40%.

[0071] Example 20: The difference from Example 18 is that the first acrylic monomer is changed to hydroxypropyl methacrylate, and the change is 40% relative to the total mass of the monomer mixture.

[0072] Example 21: The difference from Example 1 is that the cross-linking monomer is changed to divinylbenzene, and the proportion relative to the total mass of the monomer mixture is changed to 20%.

[0073] Step 1), 3.5 g of methyl methacrylate, 5 g of isooctyl acrylate (first acrylic monomer), 20% of divinylbenzene (crosslinking monomer) and 5 g of styrene (functional monomer) relative to the total mass of the monomer mixture are mixed to form a monomer mixture, 1% of benzoyl peroxide (initiator) equivalent to the mass of the monomer mixture is dissolved in the monomer mixture, and then 200 g of water and 5 g of polyvinyl alcohol (dispersant) are added to obtain a mixed solution; Comparative Example 1: The difference from Example 1 is that the monomer mixture only includes methyl methacrylate, and does not include the first acrylic monomer, the crosslinking monomer, and the functional monomer; Step 1), the monomer mixture includes 5g of methyl methacrylate, 1% of the mass of the monomer mixture of benzoyl peroxide (initiator) is dissolved in the monomer mixture, and then 200g of water and 5g of polyvinyl alcohol (dispersant) are added to obtain a mixed solution.

[0074] Comparative Example 2: The difference from Example 1 is that the monomer mixture only includes isooctyl acrylate (the first acrylic monomer) and does not contain methyl methacrylate, crosslinking monomer and functional monomer; Step 1), the monomer mixture is 5g of isooctyl acrylate (the first acrylic monomer), 1% of the mass of the monomer mixture of benzoyl peroxide (initiator) is dissolved in the monomer mixture, and then 200g of water and 5g of polyvinyl alcohol (dispersant) are added to obtain a mixed solution.

[0075] Preparation Example 1 The modified PMMA microsphere emulsion obtained in Example 1 is used to prepare a coated diaphragm, comprising: Step 1, adding 0.2 g of lauryl alcohol polyoxyethylene ether (wetting agent) into water and dissolving by ultrasonication to obtain a wetting solution; Step 2, adding 10 g of the modified PMMA microsphere emulsion obtained in Example 1 and 0.3 g of polymethacrylic acid (binder) into the wetting solution, performing ultrasonic mixing, and then filtering to obtain a modified PMMA microsphere slurry; Step 3: evenly apply the modified PMMA microsphere slurry on at least one side of the polyolefin membrane, the thickness of the modified PMMA microsphere coating is 10 μm, the thickness of the polyolefin membrane is 9 μm, the pore size of the polyolefin membrane is 0.02 μm, and a modified PMMA microsphere coated membrane is obtained by drying. The drying temperature of the drying treatment is 60° C. and the drying time is 7.5 min.

[0076] Preparation Example 2 to Preparation Example 21 The difference from Preparation 1 is that the modified PMMA microsphere emulsions obtained in Examples 2 to 21 are used to prepare the coated diaphragm.

[0077] Preparation of Comparative Examples 1 and 2 The difference from Preparation 1 is that the PMMA microsphere emulsions obtained in Comparative Example 1 and Comparative Example 2 are used to prepare the coated diaphragm.

[0078] For the pressure resistance test, the PMMA microsphere coated diaphragms prepared in the above-mentioned Preparation Examples 1 to Preparation Examples 21 and the Preparation Comparative Examples 1 and 2 were cut into 10×10 cm diaphragm slices, and loaded into an aluminum-plastic film (simulating the electrode pole piece), injected with electrolyte, packaged, put into a 60°C oven for soaking for one week, and then taken out and cut into 2.5×10 cm long strips. A pressure of 5 MPa was applied to the long strips at 65°C, and the pressure was maintained for 30 s. The morphological changes of the PMMA microsphere coated diaphragm strips before and after the pressure resistance were tested by scanning electron microscopy, and the peeling force from the aluminum-plastic film when a pressure of 3 MPa was applied to the long strips at 60°C was tested, that is, the bonding force between the PMMA microsphere coated diaphragm and the electrode pole piece, and the air permeability increase value was tested at the same time.

[0079]

[0080] Figure 4 This is a schematic diagram of a scanning electron microscope of a modified PMMA microsphere coated diaphragm of Preparation Example 5 (the cross-linking monomer is ethoxylated trimethylolpropane triacrylate, and the ratio relative to the total mass of the monomer mixture is 20%) before the withstand voltage test. Figure 5 FIG. 5 is a schematic diagram of a scanning electron microscope of the modified PMMA microsphere-coated diaphragm of Preparation Example 5 after the pressure resistance test; Figure 4 , 5 As shown, the modified PMMA microsphere coated diaphragm of Preparation Example 5 still maintains the morphology of the microspheres after the pressure resistance test, indicating that the modified PMMA microsphere coated diaphragm of Preparation Example 5 has good mechanical strength and can meet the needs of the battery.

[0081] Figure 6 This is a schematic diagram of a scanning electron microscope of the modified PMMA microsphere coated diaphragm of Preparation Example 15 (the mass of the cross-linking monomer is fixed, and the ratio of isooctyl acrylate of the acrylic monomer to the total mass of the monomer mixture is adjusted to 60%) before the withstand voltage test. Figure 7 Schematic diagram of the scanning electron microscope of the modified PMMA microsphere coated diaphragm of Preparation Example 15 after the pressure resistance test; Figure 6 , 7 As shown, the modified PMMA microsphere coated diaphragm of Preparation Example 15 still maintains the morphology of the microspheres after the pressure resistance test, indicating that the modified PMMA microsphere coated diaphragm of Preparation Example 15 has good mechanical strength and can meet the needs of the battery.

[0082] The morphology of Preparation Examples 1-4, Preparation Examples 6-14, and Preparation Examples 16-21 remained spherical after 30 seconds at 65°C and 5 MPa pressure, indicating that the mechanical strength of the PMMA microsphere-coated diaphragms of each preparation example was relatively good and could meet the needs of the battery.

[0083] Figure 8 A schematic diagram of a scanning electron microscope of a modified PMMA microsphere-coated diaphragm prepared in Comparative Example 1 (the monomer mixture includes only methyl methacrylate, without the first acrylic monomer, the cross-linking monomer, and the functional monomer) before a withstand voltage test. Fig. 9 A schematic diagram of a scanning electron microscope of a modified PMMA microsphere-coated diaphragm prepared in Comparative Example 2 (the monomer mixture only includes isooctyl acrylate of the first acrylic monomer, without methyl methacrylate, a crosslinking monomer, and a functional monomer) before a withstand voltage test. Figure 8 , Fig. 9 The microspheres of the modified PMMA microspheres coated with the diaphragm are either flattened and deformed or crushed, and the mechanical strength is relatively poor, which cannot meet the needs of the battery.

[0084] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0085] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing PMMA microsphere emulsion, characterized in that: The PMMA microspheres include a core, a linking layer and a shell, wherein the core and the shell are connected by the linking layer to form a three-dimensional network cross-linked structure, the core is a network structure formed by linking a first acrylic monomer and a cross-linking monomer, the shell is a cross-linked network formed by linking a second acrylic monomer, PMMA and the cross-linking monomer, the linking layer is formed by linking exposed double bonds of the monomers of the core or the monomers of the shell through covalent bonds, and the first oil-water partition coefficient of the first acrylic monomer is different from the second oil-water partition coefficient of the second acrylic monomer; The method comprises: In parts by mass, at a first preset temperature, 0.05 to 1.5 parts of an initiator, 50.1 to 100 parts of a monomer mixture, 100 to 600 parts of water and 0.05 to 20 parts of a dispersant are mixed and homogenized to obtain an emulsion; Passing nitrogen gas through the emulsion at the first preset temperature for a preset ventilation time; While passing nitrogen, the temperature is raised to a second preset temperature while stirring; Adding 10 to 50 parts of the second acrylic monomer to carry out polymerization reaction for a preset reaction time to obtain a modified PMMA microsphere emulsion; Wherein, the monomer mixture includes methyl methacrylate, the first acrylic monomer, the cross-linking monomer and a functional monomer.

2. The method for preparing PMMA microsphere emulsion according to claim 1, characterized in that: By weight, 0.05 to 1.5 parts of an initiator, 50.1 to 100 parts of a monomer mixture, 100 to 600 parts of water and 0.05 to 20 parts of a dispersant are mixed and homogenized to obtain an emulsion, comprising: In parts by mass, 0.05 to 1.5 parts of the initiator, 10 to 60 parts of the methyl methacrylate, 30 to 60 parts of the first acrylic monomer, 0.1 to 10 parts of the functional monomer, 100 to 600 parts of water and 0.05 to 20 parts of the dispersant are mixed, and a first homogenization is performed to obtain a pre-emulsion; 1 to 30 parts by mass of the cross-linking monomer are added to the pre-emulsion, and a second homogenization is performed to obtain an emulsion.

3. The method for preparing PMMA microsphere emulsion according to claim 2, characterized in that: The stirring speed of the first homogenization is 2500 rpm to 3000 rpm; The stirring speed of the second homogenization is 2000 rpm to 2500 rpm; The stirring speed of the stirring and heating is 150 rpm to 250 rpm; The first preset temperature is 18°C ​​to 25°C; The preset ventilation duration is 10 min to 90 min; The second preset temperature is 60°C to 90°C; The preset reaction time is 6 h to 12 h.

4. The method for preparing PMMA microsphere emulsion according to claim 1, characterized in that: The first oil-water partition coefficient of the first acrylic monomer is greater than or equal to 2.5, the second oil-water partition coefficient of the second acrylic monomer is less than 2.5, and the third oil-water partition coefficient of the cross-linking monomer is 1.5 to 2.5; The first oil-water partition coefficient of the first acrylic monomer is greater than the second oil-water partition coefficient of the second acrylic monomer, the number of carbon atoms of the first acrylic monomer is greater than or equal to 10, and the number of carbon atoms of the second acrylic monomer is greater than or equal to 4.

5. The method for preparing PMMA microsphere emulsion according to claim 1, characterized in that: The particle size D50 of the modified PMMA microsphere emulsion is 2 μm to 20 μm, and the particle size D90 is 2 μm to 50 μm.

6. The method for preparing PMMA microsphere emulsion according to claim 1, characterized in that: The first acrylic monomer is a combination of one or more of isooctyl acrylate, lauryl methacrylate, cyclohexyl methacrylate, isobornyl acrylate, and epoxy acrylate; And / or, the second acrylic monomer is a combination of one or more of isobutyl acrylate, 2-ethylbutyl acrylate, and glycidyl methacrylate; And / or, the cross-linking monomer is a combination of one or more of ethylene glycol dimethacrylate, ethoxylated trimethylolpropane triacrylate, and divinylbenzene; And / or, the dispersant is a combination of one or more of polyvinyl alcohol, sodium lauryl sulfate, polyacrylate, and polyvinyl pyrrolidone; And / or, the initiator is a combination of one or more of benzoyl peroxide and azobisisobutyronitrile; And / or, the functional monomer is a combination of one or more of styrene and silane coupling agent.

7. A method for preparing a coated diaphragm using the modified PMMA microsphere emulsion obtained by the method according to any one of claims 1 to 6, characterized in that: include: By weight, 0.2 parts of the wetting agent was added to water and ultrasonically dissolved to obtain a wetting solution; Adding 10 parts of modified PMMA microsphere emulsion and 0.3 parts of binder to the wetting solution, performing ultrasonic mixing, and filtering to obtain modified PMMA microsphere slurry; The modified PMMA microsphere slurry is uniformly coated on at least one side of the polyolefin separator, and a modified PMMA microsphere coated separator is obtained by drying. The modified PMMA microsphere coating has a thickness of 2 μm to 20 μm, the polyolefin diaphragm has a thickness of 9 μm to 20 μm, and a pore size of 0.01 μm to 0.3 μm; The drying temperature of the drying treatment is 50° C. to 70° C., and the drying time is 5 min to 10 min.

8. An electrode, characterized in that: The surface of the electrode is covered with a modified PMMA microsphere-coated diaphragm obtained by the method described in claim 7.

9. The electrode according to claim 8, characterized in that At 60° C. and 3 MPa pressure, the bonding force between the modified PMMA microsphere coated separator and the negative electrode sheet of the electrode is 2.5 N / m to 5.0 N / m.

10. A lithium battery, characterized in that: Comprising the electrode as claimed in claim 8 or 9.

Citation Information

Patent Citations

  • Nano-grade fluorescent microspheres, preparation method thereof, and purpose thereof as markers used in immunity chromatography method

    CN102604305A

  • Coated diaphragm and preparation method thereof

    CN114361706A

  • Water-based binder as well as preparation method and application thereof

    CN117487484A

  • Binder as well as preparation method and application thereof

    CN118562427A

  • Lithium ion battery positive electrode fluoride-free binder and preparation method thereof, battery positive electrode and battery

    CN118685137A

Cited By

  • Diaphragm, preparation method thereof and lithium ion battery

    CN120601069A

  • Crosslinked acrylate microsphere emulsion, preparation method thereof, battery diaphragm and lithium ion battery

    CN121159762A