Photo-thermal and electric-heating anti-icing and deicing super-hydrophobic coating and preparation method thereof
By performing low surface energy modification on epoxy resin and combining with wear-resistant hard phase and carbon materials, a solid superhydrophobic structure is built, which solves the problems of complex operation and easy failure of traditional anti-ice coatings, achieving high efficiency and convenience The light and heat and electric heat anti-icing effect is suitable for all-weather applications and reduces costs.
Patent Information
- Application Number
- CN202411330568.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional multifunctional anti-icing coatings are complex in operation, prone to failure, poor in applicability, and high in process costs, making them difficult to be suitable for large-scale construction.
By performing low-surface hydrophobic modification on epoxy resin and combining it with wear-resistant hard phase and carbon materials, a solid superhydrophobic structure is built, simplifying the process flow, avoiding hydrophobic modification of fillers, and is suitable for construction of different surfaces of objects. .
It achieves efficient and convenient photothermal and electric heat anti-icing effect, improves mechanical durability, and has a wide range of applicability. It is suitable for all-weather anti-icing and de-icing applications, reducing costs.
Smart Images

Figure CN119060608A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photothermal and electrothermal super-hydrophobic materials, and in particular relates to a photothermal and electrothermal anti-icing and de-icing super-hydrophobic coating and a preparation method thereof. Background Art
[0002] As a common phenomenon in nature, icing has a negative impact on industries such as aviation, electricity, transportation, and shipping. In severe cases, it can even cause personal injury and property damage. In order to reduce the damage caused by icing, many technologies have been applied, such as electric melting, pneumatically driven deicing, and antifreeze spraying. However, these traditional active methods have problems such as high energy consumption, difficulty in application, high labor costs, and certain harm to the environment. Superhydrophobic coatings are generally considered to be suitable anti-icing passive strategies due to their special surface structure. It has low surface energy and micro-nano roughness structure, which enables the coating to delay the freezing time of water droplets and reduce the adhesion of ice. However, superhydrophobic coatings generally only have the function of preventing icing, and there are certain limitations on the effect of preventing icing.
[0003] Patent CN105032731B provides a method for preparing an energy-saving anti-icing coating composited with a super-hydrophobic coating and a heating coating. The super-hydrophobic coating is to modify commercial fumed silica with fluorosilane, then mix it with resin in an appropriate proportion, and add thermal conductive particles at the same time; the heating coating is to evenly spray high-temperature resistant conductive glue into a fixed shape and stick aluminum foil on both ends as electrodes. Although this technology has the advantages of both coating anti-icing and electric heating anti-icing, and changes the heating method to improve thermal efficiency and achieve efficient and energy-saving anti-icing. However, this technology requires the use of long-chain silane coupling agents or fluorosilane coupling agents for hydrophobic modification of specific photothermal particle fillers, and the use of epoxy resin combined with photothermal effect for anti-icing. The process is complicated, the cost is high, and the applicability is limited.
[0004] Patent application CN118027898A discloses a method for preparing a multifunctional composite super-hydrophobic anti-icing material with efficient photothermal conversion, firstly sequentially growing mesoporous silica on the surface of photothermal particles, then sequentially immersing the sequentially grown mesoporous silica photothermal particles in low-temperature phase change materials and high-temperature phase change materials for vacuum adsorption treatment, obtaining photothermal particles with phase change function, and finally placing the photothermal particles with phase change function in anhydrous ethanol, dripping a hydrophobic modifier, and heating the reaction to obtain a composite super-hydrophobic anti-icing material. Although the material can not only prolong the ice condensation time under low temperature conditions, but also effectively regulate the temperature growth of the photothermal material, thereby reducing its possible adverse effects on the substrate; however, the technology needs to be hydrophobically modified by using fluorosilane on the nanofiller, and anti-icing is performed by using fluororesin combined with a thermal conductive coating, and the scope of application of the resulting super-hydrophobic material is limited and easy to fail.
[0005] Therefore, traditional multifunctional anti-icing coatings have disadvantages such as complex operation, easy failure, and poor adaptability. Summary of the invention
[0006] The purpose of the present invention is to overcome the problems existing in the above-mentioned prior art and to provide a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating and a preparation method thereof, which makes up for the shortcomings of traditional multifunctional anti-icing coatings that are easy to fail. The process is simple, the operation is convenient, it is suitable for large-scale construction over a large area, and it is easy to construct on the surfaces of different objects.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] The present invention provides a method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating, comprising the following steps:
[0009] S1, sequentially adding a silane coupling agent, a sodium hydroxide solution and ethanol, stirring evenly and heating in a water bath for reaction, then sequentially adding a fluorinated silane and a sodium hydroxide solution, continuing heating in a water bath for reaction, and obtaining an oligomer solution after sufficient reaction;
[0010] S2, mixing the oligomer solution obtained in step S1 with the epoxy resin, and stirring them evenly to obtain a fluorinated epoxy resin;
[0011] S3, after uniformly mixing the fluorinated epoxy resin obtained in step S2 with the wear-resistant hard phase, the carbon material, and the organic solvent, coating the mixture on a steel or glass substrate to solidify it, and after solidification, forming a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating on the surface of the substrate.
[0012] Furthermore, in step S1, the mass ratio of the silane coupling agent, sodium hydroxide solution, ethanol, fluorine-containing silane, and sodium hydroxide solution is (4-5): (0.5-0.6): (3-5): (2-2.5): (0.1-0.15).
[0013] Furthermore, in step S1, the concentration of the sodium hydroxide solution is 0.2 mol / L to 0.3 mol / L, preferably 0.25 mol / L.
[0014] Furthermore, in step S1, the water bath heating reaction is divided into two steps: the first step, after adding the silane coupling agent, sodium hydroxide solution and ethanol, heating the reaction in a water bath at 75-85°C for 0.5-1.5h, preferably heating the reaction in a water bath at 80°C for 1h; the second step, after adding the fluorinated silane and sodium hydroxide solution, heating the reaction in a water bath at 75-85°C for 3-5h, preferably heating the reaction in a water bath at 80°C for 4h.
[0015] Further, in step S1, the silane coupling agent is selected from any one of 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-aminopropyltrimethoxysilane or γ-glycidyloxypropyltrimethoxysilane; the fluorine-containing silane is selected from any one of perfluorodecyltrimethoxysilane, perfluorodecyltriethoxysilane, perfluorodecyldimethylchlorosilane, perfluorodecyltrichlorosilane, perfluorooctyltrimethoxysilane, perfluorooctylmethyldichlorosilane or perfluorooctyltrichlorosilane.
[0016] Furthermore, in step S2, the mass ratio of the oligomer solution to the epoxy resin is (0.2-0.4):(1-1.5).
[0017] Furthermore, in step S3, the mass ratio of the fluorinated epoxy resin, the wear-resistant hard phase, the carbon material, and the organic solvent is (3-4): (1-1.5): (1.2-2): (20-30).
[0018] Furthermore, in step S3, the wear-resistant hard phase is selected from at least any one of titanium nitride, titanium carbide, titanium carbonitride, silicon carbide, boron carbide, titanium boride, and titanium dioxide; the carbon material is selected from at least any one of carbon black, conductive carbon black, carbon nanotubes, acetylene black, graphene, and graphite; and the organic solvent is selected from at least any one of butyl acetate, ethyl acetate, n-hexane, toluene, and tetrahydrofuran.
[0019] Furthermore, in step S3, the curing temperature is room temperature to 80°C.
[0020] The present invention also provides a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating prepared by the preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention provides a method for preparing a photothermal and electrothermal anti-icing and de-icing super-hydrophobic coating, which uses fluorine-containing silane to perform low surface energy hydrophobic modification on epoxy resin (by grafting long-chain fluorocarbon functional groups -CF2 and -CF3 through a ring-opening reaction with epoxy groups, thereby improving the hydrophobic effect of the surface). The modified resin acts as an adhesive to bind the fillers together, enabling the super-hydrophobic coating to be firmly attached to the substrate, avoiding the reduction of the conductive performance of the carbon material after modification, and at the same time simplifying the process flow, eliminating the tedious process of hydrophobic modification of the filler.
[0023] (2) The present invention constructs a strong super-hydrophobic structure based on wear-resistant hard phase, carbon material and dual-scale composite filler, which improves the mechanical durability of the multifunctional anti-icing coating and makes up for the shortcoming that the traditional multifunctional anti-icing coating is easy to fail; at the same time, the preparation method is simple, and it can be sprayed, scraped and brushed. The process is simple and the operation is convenient. It is suitable for large-scale construction over a large area and is easy to construct on the surfaces of different objects.
[0024] (3) The present invention uses a low-cost wear-resistant hard phase as a photothermal filler and a readily available carbon material as a conductive phase. By introducing a dual-energy heating mechanism into a low-surface-energy coating, a photothermal / electrical-thermal super-hydrophobic coating for all-weather anti-icing and de-icing is developed, which solves the problem that the photothermal coating cannot actively de-ice in weak light or dark nights. Under the stimulation of light and current, the anti-icing and de-icing effects are achieved, which has great potential application value.
[0025] (4) The method of the present invention does not involve the hydrophobic modification of fillers, but focuses on the low surface energy modification of resins. From the perspective of resin modification, the resin molecular structure is grafted and modified to avoid modification of fillers. This method of resin modification is more widely applicable and can be applied to most fillers. It has a wide range of applicability and utilizes low surface energy modified resins combined with photothermal and electrothermal functions for all-weather super-hydrophobic anti-icing and de-icing applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Graphs of water contact angle and water rolling angle of epoxy resin, fluorinated epoxy resin, photothermal and electrothermal anti-icing and deicing super-hydrophobic coating in Example 1 of the present invention, wherein (a) is the water contact angle of epoxy resin, (b) is the water contact angle of fluorinated epoxy resin, (c) is the water contact angle of photothermal and electrothermal anti-icing and deicing super-hydrophobic coating, and (d) is the water rolling angle of photothermal and electrothermal anti-icing and deicing super-hydrophobic coating;
[0027] Figure 2 The figures are the delayed freezing effect diagrams of the epoxy resin, fluorinated epoxy resin, photothermal and electrothermal anti-icing and deicing super-hydrophobic coating in Example 1 of the present invention in a low temperature environment of -25°C, wherein (a) is the delayed freezing effect diagram of the epoxy resin in a low temperature environment of -25°C, (b) is the delayed freezing effect diagram of the fluorinated epoxy resin in a low temperature environment of -25°C, and (c) is the delayed freezing effect diagram of the photothermal and electrothermal anti-icing and deicing super-hydrophobic coating in a low temperature environment of -25°C;
[0028] Figure 3 The temperature change curves of the photothermal and electrothermal anti-icing and deicing super-hydrophobic coatings prepared in Example 1 of the present invention at room temperature under different light intensities and different voltage excitations, where (a) is (0.25-1) W / cm 2Temperature rise curves of photothermal and electrothermal anti-icing and deicing superhydrophobic coatings under light intensity (b) (0.1-0.25) W / cm 2 Temperature rise curves of photothermal and electrothermal anti-icing and deicing superhydrophobic coatings under electric power;
[0029] Figure 4 This is a rendering of the ice melting process of the photothermal and electrothermal anti-icing and deicing super-hydrophobic coating prepared in Example 1 of the present invention under a low temperature environment of -25°C through illumination and electrical stimulation;
[0030] Figure 5 This is a rendering of the defrosting process of the photothermal and electrothermal anti-icing and deicing super-hydrophobic coating prepared in Example 1 of the present invention under a low temperature environment of -25°C by illumination and electrical stimulation;
[0031] Figure 6 This is a contact angle diagram of the epoxy resin / acetylene black / titanium nitride coating prepared in Comparative Example 1 of the present invention and water. DETAILED DESCRIPTION
[0032] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0033] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0034] The present invention provides a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating and a preparation method thereof, the preparation method comprising the following steps:
[0035] S1, add silane coupling agent, sodium hydroxide solution and ethanol in sequence, stir evenly, heat in a water bath at 75-85°C for 0.5-1.5h, preferably heat in a water bath at 80°C for 1h, then add fluorine-containing silane and sodium hydroxide solution in sequence, continue to heat in a water bath at 75-85°C for 3-5h, preferably heat in a water bath at 80°C for 4h, and obtain an oligomer solution after sufficient reaction; the mass ratio of the silane coupling agent, sodium hydroxide solution, ethanol, fluorine-containing silane and sodium hydroxide solution is (4-5): (0.5-0.6): (3-5): (2-2.5): (0.1-0.15 ); the concentration of the sodium hydroxide solution is 0.2mol / L to 0.3mol / L, preferably 0.25mol / L; the silane coupling agent is selected from any one of 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-aminopropyltrimethoxysilane or γ-glycidyloxypropyltrimethoxysilane; the fluorine-containing silane is selected from any one of perfluorodecyltrimethoxysilane, perfluorodecyltriethoxysilane, perfluorodecyldimethylchlorosilane, perfluorodecyltrichlorosilane, perfluorooctyltrimethoxysilane, perfluorooctylmethyldichlorosilane or perfluorooctyltrichlorosilane.
[0036] S2, mixing the oligomer solution obtained in step S1 with epoxy resin, stirring evenly to obtain fluorinated epoxy resin, wherein the mass ratio of the oligomer solution to the epoxy resin is (0.2-0.4):(1-1.5).
[0037] S3, after uniformly mixing the fluorinated epoxy resin obtained in step S2 with the wear-resistant hard phase, the carbon material and the organic solvent, coating the mixture on a steel or glass substrate to cure it, the curing temperature being room temperature to 80°C, and forming a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating on the surface of the steel or glass substrate after curing; the mass ratio of the fluorinated epoxy resin, the wear-resistant hard phase, the carbon material and the organic solvent is (3-4): (1-1.5): (1.2-2): (20-30); the wear-resistant hard phase is selected from at least any one of titanium nitride, titanium carbide, titanium carbonitride, silicon carbide, boron carbide, titanium boride and titanium dioxide; the carbon material is selected from at least any one of carbon black, conductive carbon black, carbon nanotubes, acetylene black, graphene and graphite; the organic solvent is selected from at least any one of butyl acetate, ethyl acetate, n-hexane, toluene and tetrahydrofuran.
[0038] Example 1
[0039] This embodiment provides a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating and a preparation method thereof, and the specific steps are as follows:
[0040] (1) 4 g of 3-glycidyloxypropyltriethoxysilane and 0.5 g of 0.25 mol / L sodium hydroxide solution were dissolved in 3 g of ethanol, stirred evenly, and heated in a water bath at 80° C. for 1 h, then 2.5 g of perfluorodecyltriethoxysilane and 0.1 g of 0.25 mol / L sodium hydroxide solution were added thereto, and the reaction was continued by heating in a water bath at 80° C. for 4 h. After the reaction was terminated, an oligomer solution was obtained;
[0041] (2) 0.2 g of the oligomer solution and 1 g of the epoxy resin were mixed and stirred at room temperature for 15 min. After the mixture was stirred evenly, a fluorinated epoxy resin was obtained;
[0042] (3) 3 g of fluorinated epoxy resin, 1 g of titanium nitride, 1.5 g of acetylene black, and 22 g of ethyl acetate were mixed evenly and stirred for 1 hour, and then evenly coated on a steel substrate, dried and cured at 80°C to form a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating on the surface of the steel substrate.
[0043] The prepared super hydrophobic coating was subjected to performance testing, and the results are as follows:
[0044] like Figure 1 , Figure 2 As shown, the water contact angle (WCA), water rolling angle (WSA) and delayed freezing of water droplets were captured by a high-speed macro camera during the test process. The water droplet sizes used in the test were 5μL, 10μL and 10μL, respectively.
[0045] like Figure 1 As shown in the figure, the water contact angle and water rolling angle diagram of the epoxy resin, fluorinated epoxy resin, photothermal and electrothermal anti-icing and deicing superhydrophobic coating in this embodiment. In the figure, the water contact angle of the photothermal and electrothermal anti-icing and deicing superhydrophobic coating can reach 160°, and the water rolling angle is as low as 2°, while the water contact angle of ordinary epoxy resin is only 65°. Because the fluorinated epoxy resin has undergone low surface energy modification, the water contact angle is also increased to 110°.
[0046] like Figure 2 As shown in the figure, the delayed freezing effect diagram of the epoxy resin, fluorinated epoxy resin, photothermal and electric thermal anti-icing and deicing super-hydrophobic coating in this embodiment in a low temperature environment of -25°C. Compared with epoxy resin, the delayed freezing ability of fluorinated epoxy resin and photothermal and electric thermal anti-icing and deicing super-hydrophobic coating is improved by 2 times and 11 times respectively, indicating a significant improvement in the anti-icing ability of photothermal and electric thermal anti-icing and deicing super-hydrophobic coating.
[0047] like Figure 3 , Figure 4 , Figure 5As shown in the figure, in the characterization of the photothermal and electrothermal properties of the coating and the anti-icing and defrosting application, a TF900 circulating cooler is used to establish a low temperature environment for the sample. The light intensity is changed by adjusting the power output of the PLS-SXE300 xenon lamp, and the electrothermal power of the coating is adjusted by adjusting the output voltage of the RU-18-3060 DC power supply. All temperature data are recorded using a FLIR-E52 infrared thermal imager.
[0048] like Figure 3 As shown in the figure, the temperature change curves of the photothermal and electrothermal anti-icing and deicing super-hydrophobic coatings prepared in this embodiment under different light intensities and different voltage excitations at room temperature are shown in Figure 1. 2 ) light intensity, the super-hydrophobic coating can be heated up to 80°C within 5 minutes and stably maintained at 80°C; or (0.1-0.25W / cm 2 ), the super-hydrophobic coating can be heated up to 90°C within 4 minutes and stably maintained at 90°C. It can be seen that the photothermal and electrothermal anti-icing and deicing super-hydrophobic coating in this embodiment has excellent active deicing capability.
[0049] like Figure 4 , Figure 5 As shown in the figure, the effect diagram of the photothermal and electrothermal anti-icing and de-icing super-hydrophobic coating undergoing ice melting and defrosting process under a low temperature environment of -25°C through light and electrical stimulation. The super-hydrophobic coating can melt and remove 20mm×20mm×3mm ice cubes within 5 minutes, and can also melt and remove the frost layer generated on the surface of the super-hydrophobic coating at -25°C within 60 seconds, which illustrates the effectiveness and application potential of the photothermal and electrothermal anti-icing and de-icing super-hydrophobic coating in real scenarios.
[0050] Example 2
[0051] This embodiment provides a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating and a preparation method thereof, and the specific steps are as follows:
[0052] (1) 5 g of 3-aminopropyltriethoxysilane and 0.55 g of 0.2 mol / L sodium hydroxide solution were dissolved in 4 g of ethanol, stirred evenly, and heated in a water bath at 80° C. for 1.5 h. Then, 2.5 g of perfluorodecyltrimethoxysilane and 0.12 g of 0.2 mol / L sodium hydroxide solution were added thereto, and the reaction was continued by heating in a water bath at 80° C. for 3 h. After the reaction was terminated, an oligomer solution was obtained;
[0053] (2) 0.3 g of the oligomer solution and 1 g of the epoxy resin were mixed and stirred at room temperature for 15 min to obtain a fluorinated epoxy resin;
[0054] (3) 4 g of fluorinated epoxy resin, 1 g of titanium carbide, 1.5 g of conductive carbon black, and 25 g of butyl acetate were mixed and stirred for 1 h, evenly coated on a glass substrate, and dried and cured at 80°C to form a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating on the surface of the glass substrate.
[0055] Example 3
[0056] This embodiment provides a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating and a preparation method thereof, and the specific steps are as follows:
[0057] (1) 4.5 g of 3-aminopropyltrimethoxysilane and 0.6 g of 0.3 mol / L sodium hydroxide solution were dissolved in 3 g of ethanol, stirred evenly, and heated in a water bath at 80° C. for 0.5 h. Then, 2.5 g of perfluorooctyltrimethoxysilane and 0.1 g of 0.3 mol / L sodium hydroxide solution were added thereto, and the reaction was continued by heating in a water bath at 80° C. for 5 h. After the reaction was completed, an oligomer solution was obtained;
[0058] (2) 0.4 g of the oligomer solution and 1 g of the epoxy resin were mixed and stirred at room temperature for 15 min to obtain a fluorinated epoxy resin;
[0059] (3) 3.5 g of fluorinated epoxy resin, 1 g of silicon carbide, 2 g of carbon nanotubes, and 30 g of tetrahydrofuran were mixed and stirred for 1 hour, evenly coated on a steel substrate, and dried and cured at 80°C to form a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating on the surface of the steel substrate.
[0060] Comparative Example 1
[0061] Compared with Example 1, this comparative example is mostly the same, except that step (1) and step (2) are missing, and the "fluorinated epoxy resin" in step (3) is replaced by "epoxy resin". The prepared epoxy resin / acetylene black / titanium nitride coating only has photothermal and electrothermal properties, lacks the low surface energy modification process, and therefore has no superhydrophobic effect. Figure 6 As shown, the water contact angle of this coating is only 137°. During the low-temperature freezing process, it is unable to delay freezing through its superhydrophobic properties, which ultimately results in it having no anti-icing and de-icing functions.
[0062] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating, characterized in that: The steps include: S1, sequentially adding a silane coupling agent, a sodium hydroxide solution and ethanol, stirring evenly and heating in a water bath for reaction, then sequentially adding a fluorinated silane and a sodium hydroxide solution, continuing heating in a water bath for reaction, and obtaining an oligomer solution after sufficient reaction; S2, mixing the oligomer solution obtained in step S1 with the epoxy resin, and stirring them evenly to obtain a fluorinated epoxy resin; S3, after uniformly mixing the fluorinated epoxy resin obtained in step S2 with the wear-resistant hard phase, the carbon material, and the organic solvent, coating the mixture on the substrate to be treated to cure it, and after the curing is completed, a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating is formed on the surface of the substrate to be treated.
2. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S1, the mass ratio of the silane coupling agent, sodium hydroxide solution, ethanol, fluorine-containing silane, and sodium hydroxide solution is (4-5): (0.5-0.6): (3-5): (2-2.5): (0.1-0.15).
3. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S1, the concentration of the sodium hydroxide solution is 0.2 mol / L to 0.3 mol / L.
4. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S1, the water bath heating reaction is divided into two steps: the first step is to add the silane coupling agent, sodium hydroxide solution and ethanol, and then heat the reaction in a water bath at 75 to 85° C. for 0.5 to 1.5 hours; the second step is to add the fluorinated silane and sodium hydroxide solution, and then heat the reaction in a water bath at 75 to 85° C. for 3 to 5 hours.
5. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S1, the silane coupling agent is selected from any one of 3-aminopropyltriethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-aminopropyltrimethoxysilane or γ-glycidyloxypropyltrimethoxysilane; the fluorine-containing silane is selected from any one of perfluorodecyltrimethoxysilane, perfluorodecyltriethoxysilane, perfluorodecyldimethylchlorosilane, perfluorodecyltrichlorosilane, perfluorooctyltrimethoxysilane, perfluorooctylmethyldichlorosilane or perfluorooctyltrichlorosilane.
6. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S2, the mass ratio of the oligomer solution to the epoxy resin is (0.2-0.4):(1-1.5).
7. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S3, the mass ratio of the fluorinated epoxy resin, the wear-resistant hard phase, the carbon material, and the organic solvent is (3-4): (1-1.5): (1.2-2): (20-30).
8. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S3, the wear-resistant hard phase is selected from at least any one of titanium nitride, titanium carbide, titanium carbonitride, silicon carbide, boron carbide, titanium boride, and titanium dioxide; the carbon material is selected from at least any one of carbon black, conductive carbon black, carbon nanotubes, acetylene black, graphene, and graphite; and the organic solvent is selected from at least any one of butyl acetate, ethyl acetate, n-hexane, toluene, and tetrahydrofuran.
9. The method for preparing a photothermal and electrothermal anti-icing and deicing super-hydrophobic coating according to claim 1, characterized in that: In step S3, the curing temperature is room temperature to 80°C.
10. A photothermal and electrothermal anti-icing and deicing super-hydrophobic coating prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
A method for preparing an energy-saving anti-icing coating composed of a superhydrophobic coating and a heating coating.
CN105032731B
Preparation method and application of multifunctional composite super-hydrophobic anti-freezing material with efficient photothermal conversion
CN118027898A
Curable silicone coating comprising non-organotin catalyst
CN116802227A
Preparation method and application of double-size carbon-based super-hydrophobic photo-thermal deicing coating
CN117264504A
Super-hydrophobic coating based on low-surface-energy modified resin as well as preparation method and application of super-hydrophobic coating
CN118307993A
Cited By
Self-repairing anti-icing corrosion-resistant integrated coating and preparation method thereof
CN119775856A
Preparation method of photo-thermal super-amphiphobic coating
CN120364957A