Preparation method of impact-resistant high-strength polyurethane coating and application of impact-resistant high-strength polyurethane coating in stone
Through the esterification reaction of polyethylene glycol and isophorone diisocyanate and other raw materials, combined with triazine-based hyperbranched polyol and phenyl dihydroxyphosphorus phosphorus oxide, an impact-resistant high-strength polyurethane coating was prepared, solving the shortcomings of existing coating performance The problem of high strength and flame retardant performance has been improved.
Patent Information
- Application Number
- CN202411317536.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-20
AI Technical Summary
Existing polyurethane coatings have insufficient performance in terms of impact resistance and strength, and cannot meet the high requirements in fields such as stone.
Polyurethane is prepared through the esterification and neutralization process by using raw materials such as polyethylene glycol after vacuum dehydration, isophorone diisocyanate, dibutyltin bislaurate, triazine-based hyperbranched polyol, phenyl dihydroxyphosphorus oxide and other raw materials. The emulsion is added, and dispersant, wetting agent, defoaming agent, etc. are added to form impact-resistant high-strength polyurethane coating.
The prepared polyurethane coating has significantly improved impact resistance, high strength and flame retardant properties, and is suitable for high-demand application scenarios such as stone.
Smart Images

Figure CN119060624A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to a method for preparing an impact-resistant high-strength polyurethane coating and application thereof in stone. Background Art
[0002] At present, with the continuous improvement of people's living standards and living environment in my country, the demand for building stones is also increasing. Stones need to be processed before use, and then applied to the interior and exterior walls, floors, kitchens, etc. of buildings to bring beautiful and luxurious effects to the buildings. After cutting and rough polishing, the stone is sprayed with paint on its surface and cured to obtain a finely polished stone surface. With the increase in the use of stone, the requirements for the impact resistance and high strength of the paint are also increasing. Therefore, it is necessary to improve the strength and impact resistance of the paint to meet the needs of the existing market.
[0003] Polyurethane coatings have excellent mechanical strength, high chemical resistance and other properties, and are widely used in defense, chemical industry, anti-corrosion and other fields. For example, the patent with application number CN 118359988 A discloses a method for preparing a modified waterborne polyurethane coating, which uses polyurethane polyol, isocyanate monomer, cardanol waterborne chain extender and other main raw materials. The prepared polyurethane coating has good flame retardant effect and can be widely used in waterproof coatings, fire retardant coatings and other fields, but does not improve the impact resistance and strength of the polyurethane coating. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing an impact-resistant high-strength polyurethane coating and its application in stone. The prepared polyurethane coating has good impact resistance, high strength and flame retardant properties.
[0006] (II) Technical solution
[0007] A method for preparing an impact-resistant high-strength polyurethane coating, the method for preparing the impact-resistant high-strength polyurethane coating is as follows:
[0008] (1) adding the vacuum dehydrated polyethylene glycol, isophorone diisocyanate and 0.08-1% by mass of dibutyltin dilaurate to a flask, stirring and dispersing, heating to 70-80° C., reacting for 2-4 hours, adding triazine-based hyperbranched polyol thereto, continuing the reaction for 1-2 hours, and after the reaction, adding phenyl dihydroxyphosphine oxide thereto, reacting at 80-90° C. for 1-3 hours, adding triethylamine thereto for neutralization for 20-40 minutes, controlling the degree of neutralization to 60-80%, adding 25% by mass of sodium bisulfite thereto for end-capping for 1-2 hours, and finally adding deionized water thereto for emulsification for 10-20 minutes to obtain a polyurethane emulsion;
[0009] (2) Add a dispersant, a wetting agent, a defoaming agent, carbon black, and a thickener to the polyurethane emulsion, stir and disperse at a speed of 1000-1500 r / min for 30-60 minutes, then add deionized water, stir and mix evenly, and obtain an impact-resistant high-strength polyurethane coating.
[0010] Preferably, the usage ratio of the polyethylene glycol, isophorone diisocyanate, triazine-based hyperbranched polyol, and phenyl dihydroxyphosphine oxide is 100 g: (50-100) g: (10-50) g: (0.1-1) g.
[0011] Preferably, the usage ratio of the polyurethane emulsion, dispersant, wetting agent, defoamer, carbon black and thickener is 100g:(2-4.5)g:(0.5-1)g:(0.1-0.4)g:(0.3-0.8)g:(0.4-0.8)g.
[0012] Preferably, the preparation method of the triazine-based hyperbranched polyol is as follows:
[0013] S1, add tris (2-hydroxyethyl) isocyanurate, 2,2-dimethylol propionic acid, p-toluenesulfonic acid, and hydroquinone to a toluene solvent, stir and mix evenly, control the temperature to 100-120° C., react for 5-10 hours, and after the reaction is completed, cool to room temperature, adjust the pH to 7-8 with 10% sodium carbonate, wash with deionized water, and dry to obtain intermediate 1;
[0014] S2, adding intermediate 1 to toluene solvent, stirring and dispersing, then adding boron trifluoride ether catalyst and epichlorohydrin, reacting at 55-70°C for 2-5h, then adding 25% sodium hydroxide solution, heating to 75-85°C, and continuing to react for 2-4h. After the reaction is completed, distill under reduced pressure, filter, wash with deionized water, and dry to obtain intermediate 2;
[0015] S3. Add intermediate 2 to toluene solvent, stir and disperse, then add N-benzylethanolamine, raise the temperature to 80-100° C., react for 4-10 hours, and after the reaction is completed, perform vacuum distillation, wash with deionized water, and dry to obtain a triazine-based hyperbranched polyol.
[0016] Preferably, in S1, the dosage ratio of tris(2-hydroxyethyl)isocyanurate and 2,2-dimethylolpropionic acid is 1g:(1.5-2)g; the dosage of p-toluenesulfonic acid is 8-16% of the total mass of tris(2-hydroxyethyl)isocyanurate and 2,2-dimethylolpropionic acid; and the dosage of hydroquinone is 6-10% of the total mass of tris(2-hydroxyethyl)isocyanurate and 2,2-dimethylolpropionic acid.
[0017] Preferably, in S2, the usage ratio of intermediate 1, boron trifluoride etherate catalyst and epichlorohydrin is 1 g:(0.004-0.01) g:(4-4.5) g.
[0018] Preferably, in S3, the usage ratio of intermediate 2 and N-benzylethanolamine is 1 g:(0.85-1) g.
[0019] Preferably, the preparation method of the phenyl dihydroxyphosphine oxide is as follows:
[0020] Add phenylphosphonium dichloride and ethylene glycol to tetrahydrofuran solvent, stir and disperse, then add N,N-dimethylaniline, heat to 120-130°C, react for 8-12h, after the reaction, adjust the pH to 7-8 with 10% sodium bicarbonate solution, filter, distill under reduced pressure, and dry to obtain phenylphosphonium dihydroxide.
[0021] Preferably, the usage ratio of phenylphosphonium dichloride and ethylene glycol is 1g:(1-1.5)g.
[0022] Preferably, the impact-resistant high-strength polyurethane coating prepared by the preparation method is used in stone.
[0023] (III) Beneficial technical effects
[0024] The present invention uses tris (2-hydroxyethyl) isocyanurate and 2,2-dimethylol propionic acid under the catalytic reaction of p-toluenesulfonic acid to undergo an esterification reaction to obtain an intermediate 1, and uses the intermediate 1 under the catalysis of boron trifluoride ether catalyst to undergo a substitution reaction with epichlorohydrin to obtain an intermediate 2, and then reacts the intermediate with N-benzylethanolamine through a ring-opening reaction to obtain a triazine-based hyperbranched polyol. Phenyl phosphorus dichloride and ethylene glycol are used as raw materials, and N, N-dimethylaniline is used as a catalyst, and after substitution, phenyl dihydroxy phosphorus oxide is obtained. The present invention uses polyethylene glycol as a soft segment, isophorone diisocyanate as a hard segment, and phenyl dihydroxy phosphorus oxide as a chain extender, and introduces a hydroxyl-terminated triazine-based hyperbranched polyol to prepare a polyurethane emulsion, and finally adds a dispersant, a wetting agent, deionized water, etc. to the emulsion and stirs and mixes evenly to obtain an impact-resistant high-strength polyurethane coating.
[0025] The impact-resistant high-strength polyurethane coating prepared by the present invention contains a hyperbranched polyol structure, and the branched chain structure contained therein can disperse more impact energy when the polyurethane coating is impacted, thereby improving the impact resistance of the polyurethane coating. The benzene ring structure and the six-membered ring structure contained therein are used as rigid structures, and their introduction into the polyurethane coating can improve the strength and impact resistance of the polyurethane coating. In addition, the polyurethane coating prepared by the present invention contains a large amount of phosphorus and nitrogen elements, which are flame retardant elements, and their introduction into the polyurethane coating can improve the flame retardant properties of the polyurethane coating. The polyurethane coating prepared by the present invention has good flame retardant properties, impact resistance and high strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the reaction route of triazine-based hyperbranched polyols;
[0027] Figure 2 This is the reaction route of phenyl dihydroxyphosphine oxide. DETAILED DESCRIPTION
[0028] In order to make the technical problems, technical solutions and comparative effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention, rather than to limit the present invention.
[0029] The dispersant is dispersant AMP-95;
[0030] The wetting agent is wetting agent OP-10;
[0031] The defoamer is defoamer BYK-066;
[0032] The thickener is thickener TT-935.
[0033] Example 1
[0034] (1) Add 10 g of tris(2-hydroxyethyl)isocyanurate, 15 g of 2,2-dihydroxymethylpropionic acid, 2 g of p-toluenesulfonic acid, and 2 g of hydroquinone to a toluene solvent, stir and mix evenly, control the temperature to 100° C., react for 10 h, and after the reaction is completed, cool to room temperature, adjust the pH to 8 with 10% sodium carbonate, wash with deionized water, and dry to obtain intermediate 1.
[0035] (2) 6 g of intermediate 1 was added to toluene solvent, stirred and dispersed, and then 0.05 g of boron trifluoride ether catalyst and 26 g of epichlorohydrin were added thereto. The reaction was carried out at 60° C. for 4 h. Then 25% sodium hydroxide solution was added thereto, the temperature was raised to 80° C., and the reaction was continued for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, filtered, washed with deionized water, and dried to obtain intermediate 2.
[0036] (3) 20 g of intermediate 2 was added to toluene solvent, stirred and dispersed, and then 18 g of N-benzylethanolamine was added thereto. The temperature was raised to 100° C. and the reaction was carried out for 8 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a triazine-based hyperbranched polyol.
[0037] (4) Add 20 g of phenylphosphonium dichloride and 30 g of ethylene glycol to tetrahydrofuran solvent, stir and disperse, then add 5 drops of N,N-dimethylaniline, heat to 125° C., react for 8 h, and after the reaction, adjust the pH to 7 with 10% sodium bicarbonate solution, filter, distill under reduced pressure, and dry to obtain phenylphosphonium dihydroxide.
[0038] (5) 50 g of polyethylene glycol after vacuum dehydration, 25 g of isophorone diisocyanate and 0.09% by mass of dibutyltin dilaurate are added to a flask, stirred and dispersed, heated to 80° C., reacted for 2 h, and then 5 g of triazine-based hyperbranched polyol was added thereto, and the reaction was continued for 2 h. After the reaction was completed, 0.05 g of phenyl dihydroxyphosphine oxide was added thereto, and the reaction was carried out at 85° C. for 3 h. Triethylamine was added thereto for neutralization for 20 min, and the degree of neutralization was controlled to be 80%. Sodium bisulfite with a mass fraction of 25% was added thereto for end-capping for 1 h. Finally, deionized water was added thereto for emulsification for 20 min to obtain a polyurethane emulsion.
[0039] (6) Add 4.5 g of dispersant, 0.8 g of wetting agent, 0.2 g of defoaming agent, 0.6 g of carbon black, and 0.5 g of thickener to 100 g of polyurethane emulsion, stir and disperse at a speed of 1500 r / min for 40 min, then add 20 g of deionized water, stir and mix evenly to obtain an impact-resistant high-strength polyurethane coating.
[0040] Example 2
[0041] (1) 10 g of tris(2-hydroxyethyl)isocyanurate, 20 g of 2,2-dihydroxymethylpropionic acid, 4 g of p-toluenesulfonic acid, and 1.5 g of hydroquinone were added to a toluene solvent, stirred and mixed evenly, the temperature was controlled at 110° C., and the reaction was carried out for 5 h. After the reaction was completed, the mixture was cooled to room temperature, the pH was adjusted to 7 with 10% sodium carbonate, the mixture was washed with deionized water, and dried to obtain an intermediate 1.
[0042] (2) 6 g of intermediate 1 was added to toluene solvent, stirred and dispersed, and then 0.05 g of boron trifluoride ether catalyst and 25 g of epichlorohydrin were added thereto. The reaction was carried out at 60° C. for 4 h. Then 25% sodium hydroxide solution was added thereto, the temperature was raised to 80° C., and the reaction was continued for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure, filtered, washed with deionized water, and dried to obtain intermediate 2.
[0043] (3) 20 g of intermediate 2 was added to toluene solvent, stirred and dispersed, and then 18 g of N-benzylethanolamine was added thereto. The temperature was raised to 100° C. and the reaction was carried out for 8 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a triazine-based hyperbranched polyol.
[0044] (4) Add 20 g of phenylphosphonium dichloride and 25 g of ethylene glycol to tetrahydrofuran solvent, stir and disperse, then add 5 drops of N,N-dimethylaniline, heat to 120° C., react for 10 h, and after the reaction, adjust the pH to 8 with 10% sodium bicarbonate solution, filter, distill under reduced pressure, and dry to obtain phenylphosphonium dihydroxide.
[0045] (5) 50 g of polyethylene glycol after vacuum dehydration, 40 g of isophorone diisocyanate and 0.08% by mass of dibutyltin dilaurate are added to a flask, stirred and dispersed, heated to 70° C., reacted for 4 h, and then 10 g of triazine-based hyperbranched polyol was added thereto, and the reaction was continued for 1 h. After the reaction was completed, 0.2 g of phenyl dihydroxyphosphine oxide was added thereto, and the reaction was carried out at 90° C. for 1 h. Triethylamine was added thereto for neutralization for 40 min, and the degree of neutralization was controlled to be 60%. Sodium bisulfite with a mass fraction of 25% was added thereto for end-capping for 2 h. Finally, deionized water was added thereto for emulsification for 10 min to obtain a polyurethane emulsion.
[0046] (6) Add 3.5 g of dispersant, 0.8 g of wetting agent, 0.4 g of defoaming agent, 0.5 g of carbon black, and 0.6 g of thickener to 100 g of polyurethane emulsion, stir and disperse at a speed of 1500 r / min for 50 min, then add 16 g of deionized water, stir and mix evenly to obtain an impact-resistant high-strength polyurethane coating.
[0047] Example 3
[0048] (1) 10 g of tris(2-hydroxyethyl)isocyanurate, 18 g of 2,2-dihydroxymethylpropionic acid, 3 g of p-toluenesulfonic acid, and 2.5 g of hydroquinone were added to a toluene solvent, stirred and mixed evenly, and the temperature was controlled at 120° C. The reaction was carried out for 6 h. After the reaction was completed, the mixture was cooled to room temperature, the pH was adjusted to 8 with 10% sodium carbonate, the mixture was washed with deionized water, and dried to obtain an intermediate 1.
[0049] (2) 6 g of intermediate 1 was added to toluene solvent, stirred and dispersed, and then 0.024 g of boron trifluoride ether catalyst and 25 g of epichlorohydrin were added thereto, and the reaction was carried out at 60° C. for 5 h. Then 25% sodium hydroxide solution was added thereto, and the temperature was raised to 80° C. and the reaction was continued for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, filtered, washed with deionized water, and dried to obtain intermediate 2.
[0050] (3) 20 g of intermediate 2 was added to toluene solvent, stirred and dispersed, and then 20 g of N-benzylethanolamine was added thereto, and the temperature was raised to 80° C. and reacted for 10 h. After the reaction was completed, it was distilled under reduced pressure, washed with deionized water, and dried to obtain a triazine-based hyperbranched polyol.
[0051] (4) Add 20 g of phenylphosphonium dichloride and 20 g of ethylene glycol to tetrahydrofuran solvent, stir and disperse, then add 5 drops of N,N-dimethylaniline, heat to 130° C., react for 12 h, and after the reaction, adjust the pH to 7 with 10% sodium bicarbonate solution, filter, distill under reduced pressure, and dry to obtain phenylphosphonium dihydroxide.
[0052] (5) 50 g of polyethylene glycol after vacuum dehydration, 50 g of isophorone diisocyanate and 1% by mass of dibutyltin dilaurate are added to a flask, stirred and dispersed, heated to 75° C., reacted for 3 h, and then 15 g of triazine-based hyperbranched polyol was added thereto, and the reaction was continued for 1 h. After the reaction was completed, 0.3 g of phenyl dihydroxyphosphine oxide was added thereto, and the reaction was carried out at 80° C. for 2 h. Triethylamine was added thereto for neutralization for 30 min, and the degree of neutralization was controlled to be 70%. Sodium bisulfite with a mass fraction of 25% was added thereto for end-capping for 2 h. Finally, deionized water was added thereto for emulsification for 10 min to obtain a polyurethane emulsion.
[0053] (6) Add 2 g of dispersant, 1 g of wetting agent, 0.1 g of defoaming agent, 0.5 g of carbon black, and 0.8 g of thickener to 100 g of polyurethane emulsion, stir and disperse at a speed of 1500 r / min for 30 min, then add 20 g of deionized water, stir and mix evenly to obtain an impact-resistant high-strength polyurethane coating.
[0054] Example 4
[0055] (1) 10 g of tris(2-hydroxyethyl)isocyanurate, 18 g of 2,2-dihydroxymethylpropionic acid, 2 g of p-toluenesulfonic acid, and 2 g of hydroquinone were added to a toluene solvent, stirred and mixed evenly, and the temperature was controlled at 115° C. The reaction was performed for 8 h. After the reaction was completed, the mixture was cooled to room temperature, the pH was adjusted to 7 with 10% sodium carbonate, the mixture was washed with deionized water, and dried to obtain an intermediate 1.
[0056] (2) 6 g of intermediate 1 was added to toluene solvent, stirred and dispersed, and then 0.04 g of boron trifluoride ether catalyst and 24 g of epichlorohydrin were added thereto. The reaction was carried out at 70° C. for 2 h. Then 25% sodium hydroxide solution was added thereto, the temperature was raised to 85° C., and the reaction was continued for 2 h. After the reaction was completed, the mixture was distilled under reduced pressure, filtered, washed with deionized water, and dried to obtain intermediate 2.
[0057] (3) 20 g of intermediate 2 was added to toluene solvent, stirred and dispersed, and then 17 g of N-benzylethanolamine was added thereto. The temperature was raised to 90° C. and the reaction was carried out for 6 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a triazine-based hyperbranched polyol.
[0058] (4) Add 20 g of phenylphosphonium dichloride and 25 g of ethylene glycol to tetrahydrofuran solvent, stir and disperse, then add 5 drops of N,N-dimethylaniline, heat to 125° C., react for 10 h, and after the reaction, adjust the pH to 8 with 10% sodium bicarbonate solution, filter, distill under reduced pressure, and dry to obtain phenylphosphonium dihydroxide.
[0059] (5) 50 g of polyethylene glycol after vacuum dehydration, 40 g of isophorone diisocyanate and 0.1% by mass of dibutyltin dilaurate are added to a flask, stirred and dispersed, heated to 75° C., reacted for 2 h, and then 20 g of triazine-based hyperbranched polyol was added thereto, and the reaction was continued for 2 h. After the reaction was completed, 0.4 g of phenyl dihydroxyphosphine oxide was added thereto, and the reaction was carried out at 85° C. for 3 h. Triethylamine was added thereto for neutralization for 20 min, and the degree of neutralization was controlled to be 80%. Sodium bisulfite with a mass fraction of 25% was added thereto for end-capping for 1 h. Finally, deionized water was added thereto for emulsification for 15 min to obtain a polyurethane emulsion.
[0060] (6) Add 3 g of dispersant, 0.5 g of wetting agent, 0.2 g of defoaming agent, 0.3 g of carbon black, and 0.5 g of thickener to 100 g of polyurethane emulsion, stir and disperse at a speed of 1000 r / min for 50 min, then add 15 g of deionized water, stir and mix evenly to obtain an impact-resistant high-strength polyurethane coating.
[0061] Example 5
[0062] (1) 10 g of tris(2-hydroxyethyl)isocyanurate, 18 g of 2,2-dihydroxymethylpropionic acid, 3 g of p-toluenesulfonic acid, and 2 g of hydroquinone were added to a toluene solvent, stirred and mixed evenly, and the temperature was controlled at 110° C. to react for 8 h. After the reaction was completed, the mixture was cooled to room temperature, the pH was adjusted to 8 with 10% sodium carbonate, the mixture was washed with deionized water, and dried to obtain an intermediate 1.
[0063] (2) 6 g of intermediate 1 was added to toluene solvent, stirred and dispersed, and then 0.06 g of boron trifluoride ether catalyst and 27 g of epichlorohydrin were added thereto. The reaction was carried out at 55° C. for 4 h. Then 25% sodium hydroxide solution was added thereto, the temperature was raised to 75° C., and the reaction was continued for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure, filtered, washed with deionized water, and dried to obtain intermediate 2.
[0064] (3) 20 g of intermediate 2 was added to toluene solvent, stirred and dispersed, and then 18 g of N-benzylethanolamine was added thereto. The temperature was raised to 100° C. and the reaction was carried out for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a triazine-based hyperbranched polyol.
[0065] (4) Add 20 g of phenylphosphonium dichloride and 25 g of ethylene glycol to tetrahydrofuran solvent, stir and disperse, then add 5 drops of N,N-dimethylaniline, heat to 125° C., react for 10 h, and after the reaction, adjust the pH to 7 with 10% sodium bicarbonate solution, filter, distill under reduced pressure, and dry to obtain phenylphosphonium dihydroxide.
[0066] (5) 50 g of polyethylene glycol after vacuum dehydration, 30 g of isophorone diisocyanate and 0.08% by mass of dibutyltin dilaurate are added to a flask, stirred and dispersed, heated to 75° C., reacted for 4 h, and then 25 g of triazine-based hyperbranched polyol was added thereto, and the reaction was continued for 1.5 h. After the reaction was completed, 0.5 g of phenyl dihydroxyphosphine oxide was added thereto, and the reaction was carried out at 85° C. for 3 h. Triethylamine was added thereto for neutralization for 40 min, and the degree of neutralization was controlled to be 80%. Sodium bisulfite with a mass fraction of 25% was added thereto for end-capping for 1 h. Finally, deionized water was added thereto for emulsification for 15 min to obtain a polyurethane emulsion.
[0067] (6) Add 4.5 g of dispersant, 0.8 g of wetting agent, 0.4 g of defoaming agent, 0.8 g of carbon black, and 0.4 g of thickener to 100 g of polyurethane emulsion, stir and disperse at a speed of 1200 r / min for 60 min, then add 10 g of deionized water, stir and mix evenly to obtain an impact-resistant high-strength polyurethane coating.
[0068] Comparative Example 1
[0069] The difference between this comparative example and Example 1 is that in step (5), diethylene glycol is used instead of phenyl dihydroxyphosphine oxide.
[0070] The coating was scraped onto a glass plate to obtain a coating with a thickness of 1.5 mm. The coating was formed at 23° C. and a relative humidity of 60%, cured for 4 days, demoulded, and then cured for 3 days under standard experimental conditions to obtain a coating film.
[0071] Refer to GB / T16777-1997 to test the tensile strength of the coating.
[0072] Refer to GB / T 1732-2020 to test the impact resistance of the coating.
[0073] Refer to GB / T2406 to test the limiting oxygen index of the coating.
[0074] Table 1:
[0075] Tensile strength(MPa) Impact resistance (kg / cm) Oxygen index (%) Example 1 5.46 50 26 Example 2 6.03 50 27 Example 3 7.16 50 29 Example 4 7.92 50 31 Example 5 8.39 50 32 Comparative Example 1 5.04 45 23
[0076] It can be seen from the table that the polyurethane coating prepared by the present invention has good impact resistance, strength and flame retardancy.
[0077] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A method for preparing an impact-resistant high-strength polyurethane coating, characterized in that: The preparation method of the impact-resistant high-strength polyurethane coating is as follows: (1) Add the vacuum dehydrated polyethylene glycol, isophorone diisocyanate, and 0.08-1% by mass of dibutyltin dilaurate into a flask, stir and disperse, heat to 70-80° C., react for 2-4 hours, then add triazine-based hyperbranched polyol, continue to react for 1-2 hours, and after the reaction is completed, add phenyl dihydroxyphosphine oxide, react at 80-90° C. for 1-3 hours, then add triethylamine for neutralization for 20- 40min, controlling the neutralization degree to be 60-80%, adding 25% by mass of sodium bisulfite to block the emulsion for 1-2h, and finally adding deionized water to emulsify the emulsion for 10-20min to obtain a polyurethane emulsion, wherein the polyethylene glycol, isophorone diisocyanate, triazine-based hyperbranched polyol, and phenyl dihydroxyphosphine oxide are used in a ratio of 100g:(50-100)g:(10-50)g:(0.1-1)g; (2) Add a dispersant, a wetting agent, a defoaming agent, carbon black, and a thickener to the polyurethane emulsion, stir and disperse at a speed of 1000-1500 r / min for 30-60 minutes, then add deionized water, stir and mix evenly, and obtain an impact-resistant high-strength polyurethane coating.
2. The method for preparing the impact-resistant high-strength polyurethane coating according to claim 1, characterized in that: The usage ratio of the polyurethane emulsion, dispersant, wetting agent, defoamer, carbon black and thickener is 100g:(2-4.5)g:(0.5-1)g:(0.1-0.4)g:(0.3-0.8)g:(0.4-0.8)g.
3. The method for preparing the impact-resistant high-strength polyurethane coating according to claim 1, characterized in that: The preparation method of the triazine-based hyperbranched polyol is as follows: S1, add tris (2-hydroxyethyl) isocyanurate, 2,2-dimethylol propionic acid, p-toluenesulfonic acid, and hydroquinone to a toluene solvent, stir and mix evenly, control the temperature to 100-120° C., react for 5-10 hours, and after the reaction is completed, cool to room temperature, adjust the pH to 7-8 with 10% sodium carbonate, wash with deionized water, and dry to obtain intermediate 1; S2, adding intermediate 1 to toluene solvent, stirring and dispersing, then adding boron trifluoride ether catalyst and epichlorohydrin, reacting at 55-70°C for 2-5h, then adding 25% sodium hydroxide solution, heating to 75-85°C, and continuing to react for 2-4h. After the reaction is completed, distill under reduced pressure, filter, wash with deionized water, and dry to obtain intermediate 2; S3. Add intermediate 2 to toluene solvent, stir and disperse, then add N-benzylethanolamine, raise the temperature to 80-100° C., react for 4-10 hours, and after the reaction is completed, perform vacuum distillation, wash with deionized water, and dry to obtain a triazine-based hyperbranched polyol.
4. The method for preparing the impact-resistant high-strength polyurethane coating according to claim 3, characterized in that: In S1, the dosage ratio of tris(2-hydroxyethyl)isocyanurate and 2,2-dimethylolpropionic acid is 1g:(1.5-2)g; the dosage of p-toluenesulfonic acid is 8-16% of the total mass of tris(2-hydroxyethyl)isocyanurate and 2,2-dimethylolpropionic acid; and the dosage of hydroquinone is 6-10% of the total mass of tris(2-hydroxyethyl)isocyanurate and 2,2-dimethylolpropionic acid.
5. The method for preparing the impact-resistant high-strength polyurethane coating according to claim 3, characterized in that: In S2, the usage ratio of the intermediate 1, the boron trifluoride etherate catalyst, and epichlorohydrin is 1 g:(0.004-0.01) g:(4-4.5) g.
6. The method for preparing the impact-resistant high-strength polyurethane coating according to claim 3, characterized in that: In the S3, the usage ratio of the intermediate 2 and N-benzylethanolamine is 1 g:(0.85-1) g.
7. The method for preparing the impact-resistant high-strength polyurethane coating according to claim 1, characterized in that: The preparation method of the phenyl dihydroxyphosphine oxide is as follows: Add phenylphosphonium dichloride and ethylene glycol to tetrahydrofuran solvent, stir and disperse, then add N,N-dimethylaniline, heat to 120-130°C, react for 8-12h, after the reaction, adjust the pH to 7-8 with 10% sodium bicarbonate solution, filter, distill under reduced pressure, and dry to obtain phenylphosphonium dihydroxide.
8. The method for preparing the impact-resistant high-strength polyurethane coating according to claim 7, characterized in that: The usage ratio of the phenylphosphonium dichloride and ethylene glycol is 1g:(1-1.5)g.
9. Application of the impact-resistant high-strength polyurethane coating prepared by the preparation method according to claim 1 in stone.
Citation Information
Patent Citations
Preparation method of modified waterborne polyurethane coating
CN118359988A
Hyperbranched waterborne polyurethane with isocyanurate as core and preparation method thereof
CN105440259A
Halogen-free high-flame-retardant cable material and preparation method thereof
CN116874999A
Cited By
Preparation method of antibacterial wear-resistant waterborne polyurethane coating
CN119639328A
Hyperbranched polyurethane with high tensile strength and preparation method thereof
CN120904426A
A hyperbranched polyurethane with high tensile strength and its preparation method
CN120904426B
Sunscreen energy-saving glass based on silica gel defoaming agent and preparation method of sunscreen energy-saving glass
CN121494349A
Sun protection energy-saving glass based on silicone gel defoaming agent and preparation method thereof
CN121494349B