Protein adhesion super-smooth coating and application thereof

The phase-transform adhesion coating formed by reducing proteins is modified by reducing agents and filled with lubricants, solving the stability of the superslip coating when the substrate interacts with the aqueous solution, and achieving the formation of resistance on the surface of various materials Dirt, ice and corrosion-resistant ultra-slip coatings are suitable for a variety of application scenarios.

CN119060634APending Publication Date: 2024-12-03SHAANXI NORMAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411259439.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing ultraslip coatings are prone to degradation when the substrate interacts with the aqueous solution, and rely on fragile porous structure and weak adhesion, resulting in the depletion of the lubricating layer, making it difficult to prepare a stable ultraslip coating.

Method used

The phase-transform adhesion coating obtained by reducing proteins is modified by reducing agents and filled with lubricant to form a tightly arranged protein adhesion superslip coating, and the stability with substrate and micro-nano particles is achieved using a variety of functional groups of the protein. Combined, it forms a coating that is resistant to stain, ice and corrosion.

Benefits of technology

It realizes chemical and mechanical stability of adhesion on the surface of various materials, provides anti-fouling, ice and corrosion resistance, and is simple, green and non-toxic, and can be self-cleaned without detergent. It is suitable for food transportation Pipelines, food processing equipment and frozen food processing tables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060634A_ABST
    Figure CN119060634A_ABST
Patent Text Reader

Abstract

The invention discloses a protein adhesion super-smooth coating and application thereof. The super-smooth coating is formed by modifying micro-nano particles on a phase transformation adhesion coating obtained by reducing protein with a reducing agent and filling the phase transformation adhesion coating with a lubricant. The coating is simple in preparation method, can be adhered to the surface of any material, and has good mechanical stability. The super-smooth coating can modify a liquid food material transportation pipeline, and the obtained pipeline can reduce resistance and resist pollution; modifying the surface of the frozen food processing equipment to obtain an ice adhesion resistant surface; the food processing apparatus is modified to obtain an anti-corrosion and anti-fouling surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of natural polymer materials and ecological environment materials, and specifically relates to an ultra-slip coating formed by modifying micro-nano particles on a protein phase transition adhesion coating and filling a lubricant. Background Art

[0002] Super-slippery coatings are inspired by pitcher plants and consist of a micro-nanostructured substrate and a lubricant, which solves the limitations of super-hydrophobic surfaces. As a new coating strategy for surface modification, liquid-infused super-slippery coatings have received a lot of attention in the past few years. The process of injecting lubricants into porous structures is the most critical step in the preparation of liquid-infused super-slippery coatings. Most reports currently use lubricating oils to impregnate micro / nanoporous structures, which use the capillary force of the porous structure of the substrate and the surface tension of the lubricant as the driving force to inject the lubricant into the porous structure. The lubricant layer reduces the interaction force between external substances and the substrate, allowing contaminants to slide off easily and significantly reducing the adhesion of surface stains. Compared with super-hydrophobic surfaces, liquid-infused super-slippery surfaces have lower contact angle hysteresis, sometimes even below 5°, so their applications in anti-corrosion, anti-icing, medical devices, and self-healing are gaining more and more attention.

[0003] However, liquid-infused super-lubricant coatings also face great challenges, such as their reliance on fragile hierarchical porous structures and the potential degradation when the micro-nanostructure substrate interacts with the aqueous solution. In addition, the weak adhesion between the micro-nanostructure and the substrate can also lead to the depletion of the lubricating layer. Solving these problems is crucial for the rapid and direct preparation of stable super-lubricant coatings.

[0004] Polydopamine systems inspired by mussel marine organisms are often used as modified coatings on material surfaces to achieve stable adhesion to substrates and have been applied as interlayers to fabricate superslip coatings. In addition, phenol-rich tannic acid systems utilize the abundant phenolic hydroxyl groups of tannic acid to form a slippery coating by reacting with metal cations (Fe 3+ ) to stabilize the adhesion with the material surface. However, this method still has some disadvantages, such as instability and coloration problems, especially in oxidative and alkaline environments. Summary of the invention

[0005] The purpose of the present invention is to provide a protein-adhesive super-slippery coating which has a simple preparation method, can be adhered to the surface of any substrate, has good anti-fouling performance, anti-icing performance and anti-metal corrosion performance, and has excellent mechanical stability.

[0006] For the above purpose, the protein adhesion super-slippery coating used in the present invention is a coating formed by modifying micro-nano particles on a phase transition adhesion coating obtained by reducing protein with a reducing agent and filling it with a lubricant, wherein the micro-nano particles have a closely arranged micro-nano structure.

[0007] The above-mentioned protein includes any one of lysozyme, soy protein, whey protein, lactoferrin, legumin, serum albumin, fibrinogen, zein, collagen, barley protein, gluten, kidney bean protein, keratin, casein, pepsin, myoglobin, lactalbumin, β-lactoglobulin, collagen, albumin, collagen, etc.

[0008] The reducing agent mentioned above includes any one of cysteine, mercaptoethanol, tris(2-carboxyethyl)phosphine hydrochloride, glutathione, dithiothreitol and the like.

[0009] The above-mentioned micro-nano particles include any one of silicon dioxide, aluminum oxide, silicon carbide, silicon nitride, titanium oxide and the like.

[0010] The lubricant includes any one of silicone oil, perfluoropolyether, perfluorodecahydronaphthalene, castor oil, coconut oil, corn oil, mustard oil, olive oil, palm oil, rapeseed oil, soybean oil, cottonseed oil, paraffin oil, etc.

[0011] The preparation method of the protein adhesion super-slippery coating of the present invention comprises the following steps: adjusting a 4-hydroxyethylpiperazineethanesulfonic acid buffer solution containing 1 to 100 mg / mL of a reducing agent to a pH of 4 to 10 with NaOH, and then uniformly mixing the 4-hydroxyethylpiperazineethanesulfonic acid buffer solution containing 1 to 100 mg / mL of a protein at a volume ratio of 1:1 to obtain a mixed solution; dip-coating, spray-coating or drop-coating the obtained mixed solution on the surface of any material, and incubating at room temperature for 0.1 to 5 hours to modify the protein phase transition adhesion coating on the surface of the material; dip-coating, spray-coating or spin-coating a micro-nano particle dispersion on the protein phase transition adhesion coating to obtain a protein phase transition adhesion coating modified with micro-nano particles; and filling a lubricant in the micro-nano structure of the micro-nano particles to obtain a protein adhesion super-slippery coating.

[0012] In the above preparation method, preferably, a 1-10 mg / mL reducing agent 4-hydroxyethylpiperazineethanesulfonic acid buffer solution is adjusted to a pH of 6-9 with NaOH, and then mixed with a 1-10 mg / mL protein 4-hydroxyethylpiperazineethanesulfonic acid buffer solution in a volume ratio of 1:1 to obtain a mixed solution.

[0013] In the above preparation method, the material includes any one of common experimental materials, materials for food processing equipment, and material transportation pipeline materials, specifically including any one of silicon, glass, quartz, mica, pottery, porcelain, polymethyl methacrylate, polystyrene, polyethylene terephthalate, polycarbonate, polyvinyl chloride, polyvinylidene chloride, polyamide, polyurethane, phenolic resin, rubber, polypropylene, polyethylene, various alloy materials, etc.

[0014] The protein adhesion super-slippery coating provided by the present invention can be used in any of the following production and life applications:

[0015] (1) Application in the preparation of self-cleaning liquid food transportation pipelines;

[0016] (2) Application in the preparation of food processing materials that resist microbial and protein adhesion;

[0017] (3) Application in the preparation of drag-reducing coatings for liquid food transportation pipelines;

[0018] (4) Application in food processing equipment that resists metal corrosion;

[0019] (5) Application in the preparation of anti-ice adhesion.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention utilizes a reducing agent to effectively reduce the disulfide bonds of proteins to induce rapid protein self-assembly to obtain a phase change adhesion coating. The obtained phase change adhesion coating can adhere to the surface of various materials and has good chemical stability and mechanical stability. Compared with the dopamine system, the protein phase change adhesion coating, as a stable adhesive layer, presents various types of functional groups, which can achieve stable and reliable multiple bonds with the underlying material and the top layer of micro-nanoparticles. The protein phase change adhesion coating is used as an adhesive to stabilize the micro-nanoparticles on various materials to form an ultra-slip coating with anti-fouling, anti-icing and anti-corrosion properties. The ultra-slip coating has excellent mechanical stability, and the preparation method is simple and green, and the obtained coating is non-toxic and harmless, which can solve the problems of difficult cleaning, icing and metal corrosion in production. The details are as follows:

[0022] (1) The super-slip coating can resist various mechanical treatments and has excellent mechanical stability;

[0023] (2) The super-slip coating can be used to modify food material transportation pipelines to obtain self-cleaning pipelines that can resist the adhesion of various liquid foods (cola, juice, milk, tea, coffee, yogurt, etc.) without the use of detergents;

[0024] (3) The super-slip coating can be used to modify food processing equipment for antimicrobial and protein adhesion, thereby obtaining an antimicrobial adhesion surface, which is beneficial to food safety;

[0025] (4) The super-slip coating can also be used to modify metal materials to obtain corrosion-resistant metal materials;

[0026] (5) The ultra-slip coating can also be used to modify frozen food processing tables to obtain food processing tables that are resistant to ice adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is an atomic force microscope scan of the lysozyme phase change adhesion coating prepared in Example 1.

[0028] Figure 2 This is an atomic force microscope scan of the lysozyme phase change adhesion coating modified with silica in Example 1.

[0029] Figure 3 It is the change in contact angle of the protein-adhesive super-slippery coating after ultrasonic treatment in Example 2.

[0030] Figure 4 is the contact angle of the protein-adhesive super-slippery coating in Example 2 after being soaked in hydrochloric acid at pH=2.

[0031] Figure 5 is the contact angle of the protein-adhesive super-slippery coating in Example 2 after being immersed in a sodium hydroxide aqueous solution with a pH of 12.

[0032] Figure 6 is the contact angle of the protein-adherent super-slippery coating in Example 2 after centrifugation at different speeds.

[0033] Figure 7 It is a comparison of the anti-fouling performance of the protein-adhered super-slippery coating and the super-slippery coating without protein adhesion in Example 2 after 50 frictions.

[0034] Figure 8 This is the situation of the glass sheet modified with the protein adhesion super-slippery coating and the blank glass sheet in Example 9 against liquid food adhesion.

[0035] Fig. 9 This is a laser confocal image of the protein-adhered super-slippery coating surface resisting the adhesion of Escherichia coli in Example 9.

[0036] Fig.10 This is a laser confocal image of the protein-adhesive super-slippery coating surface in Example 9 that resists the adhesion of Staphylococcus aureus.

[0037] Fig.11 This is the case of the protein-adhesive super-slippery coating in Example 9 resisting milk adhesion.

[0038] Fig.12 The stainless steel sheet modified with the protein-adhesive super-slippery coating in Example 10 resists ice adhesion.

[0039] Fig.13 It is the iron sheet modified by the protein adhesion super-slip coating in Example 11 that delays corrosion in salt spray. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to these embodiments.

[0041] Example 1

[0042] 20 mg of L-cysteine ​​was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4 and the pH was adjusted to 7.5 with a 5 mol / L sodium hydroxide aqueous solution. 20 mg of lysozyme was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and the two solutions were mixed evenly to obtain a mixed solution. A silicon wafer was immersed in the mixed solution and cultured at room temperature for 1 hour to form a lysozyme phase transition adhesion coating on the surface of the silicon wafer (see Figure 1 ); then the lysozyme phase transition adhesion coating was immersed in a silica sol having a mass concentration of 3% for 5 min to obtain a lysozyme phase transition adhesion coating modified with silica (see Figure 2 ), and then fill the micro-nano structure of silica with silicone oil to obtain a silicon wafer modified with a protein-adhesive super-slippery coating. Figure 1 This indicates that after the phase transition, lysozyme forms a nanofilm composed of oligomers with a size of 50 nm. Figure 2 This indicates that silica nanoparticles are tightly assembled on the lysozyme phase-change adhesion coating.

[0043] Example 2

[0044] 50 mg of L-cysteine ​​is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the pH value is adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution; 50 mg of lysozyme is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and then the two solutions are evenly mixed to obtain a mixed solution; a polyethylene terephthalate material is immersed in the mixed solution, and cultured at room temperature for 0.5 h to form a lysozyme phase transition adhesion coating on the surface of the polyethylene terephthalate material; then the lysozyme phase transition adhesion coating is immersed in a silica sol with a mass concentration of 3% for 10 minutes to obtain a lysozyme phase transition adhesion coating modified with silica, and then the micro-nano structure of silica is filled with paraffin oil to obtain a polyethylene terephthalate material modified with a protein adhesion super-slippery coating.

[0045] The polyethylene terephthalate material modified with the protein adhesion super-slippery coating was ultrasonically treated in a 400 W ultrasonic cleaner for 20 min. Figure 3 The protein adhesion super-slippery coating did not fall off and the contact angle remained unchanged. The polyethylene terephthalate material modified with the protein adhesion super-slippery coating was immersed in hydrochloric acid at pH = 2 for 4 days. Figure 4 The contact angle and rolling angle of the protein adhesion super-slippery coating did not change significantly. The polyethylene terephthalate material modified with the protein adhesion super-slippery coating was immersed in a sodium hydroxide aqueous solution with a pH of 12 for 4 days. Figure 5 The contact angle and rolling angle of the protein adhesion super-slippery coating did not change significantly. The polyethylene terephthalate material modified with the protein adhesion super-slippery coating was centrifuged at different speeds. Figure 6 It shows that there is no significant change in the contact angle and sliding angle of the protein-adhesive super-slippery coating. Figure 7 The results show that the polyethylene terephthalate material modified with the protein adhesion super-slippery coating can still resist milk adhesion after 50 frictions (400-grit sandpaper), while the super-slippery coating without the protein adhesion coating (the polyethylene terephthalate material is directly immersed in a silica sol with a mass concentration of 3% for 10 minutes, and then the micro-nano structure of silica is filled with paraffin oil) will stick to milk after 50 frictions. The above data show that the protein adhesion super-slippery coating has excellent mechanical stability, chemical stability and adhesion stability.

[0046] Example 3

[0047] 30 mg of L-cysteine ​​was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the pH value was adjusted to 9 with a 5 mol / L sodium hydroxide aqueous solution; 30 mg of lysozyme was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and then the two solutions were evenly mixed to obtain a mixed solution; a copper substrate was immersed in the mixed solution, and cultured at room temperature for 0.5 h to form a lysozyme phase transition adhesion coating on the surface of the copper substrate; then the lysozyme phase transition adhesion coating was immersed in a silica sol with a mass concentration of 3% for 10 minutes to obtain a lysozyme phase transition adhesion coating modified with silica, and then the micro-nano structure of silica was filled with silicone oil to obtain a copper substrate modified with a protein adhesion super-slippery coating.

[0048] Example 4

[0049] 143 mg of tris(2-carboxyethyl)phosphine hydrochloride is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and the pH is adjusted to 7 with a 5 mol / L sodium hydroxide aqueous solution, 50 mg of lysozyme is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and then the two solutions are evenly mixed to obtain a mixed solution; a polyethylene material is immersed in the mixed solution and cultured at room temperature for 0.5 h to form a lysozyme phase transition adhesion coating on the surface of the polyethylene material; then the lysozyme phase transition adhesion coating is immersed in a silica sol with a mass concentration of 3% for 5 minutes to obtain a lysozyme phase transition adhesion coating modified with silica, and then the micro-nano structure of silica is filled with silicone oil to obtain a polyethylene material modified with a protein adhesion super-slippery coating.

[0050] Example 5

[0051] 143 mg of tris(2-carboxyethyl)phosphine hydrochloride is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and the pH is adjusted to 6 with a 5 mol / L sodium hydroxide aqueous solution, 20 mg of lysozyme is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and then the two solutions are evenly mixed to obtain a mixed solution; a stainless steel sheet is immersed in the mixed solution and cultured at room temperature for 2 hours to form a lysozyme phase transition adhesion coating on the surface of the stainless steel sheet; then the lysozyme phase transition adhesion coating is immersed in a silica sol with a mass concentration of 3% for 5 minutes to obtain a lysozyme phase transition adhesion coating modified with silica, and then the micro-nano structure of silica is filled with silicone oil to obtain a stainless steel sheet modified with a protein adhesion super-slippery coating.

[0052] Example 6

[0053] 143 mg of tri(2-carboxyethyl)phosphine hydrochloride is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the pH value is adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution; 20 mg of bovine serum albumin is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and then the two solutions are evenly mixed to obtain a mixed solution; a polyurethane material is immersed in the mixed solution, and cultured at room temperature for 1 hour to form a bovine serum albumin phase transition adhesion coating on the surface of the polyurethane material; then the bovine serum albumin phase transition adhesion coating is immersed in a silica sol with a mass concentration of 3% for 5 minutes to obtain a lysozyme phase transition adhesion coating modified with silica; and then the micro-nano structure of silica is filled with silicone oil to obtain a polyurethane material modified with a protein adhesion super-slippery coating.

[0054] Example 7

[0055] 20 mg of glutathione is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and the pH is adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution; 20 mg of lysozyme is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and then the two solutions are evenly mixed to obtain a mixed solution; a stainless steel material is immersed in the mixed solution and cultured at room temperature for 1 hour to form a lysozyme phase transition adhesion coating on the surface of the stainless steel material; then the lysozyme phase transition adhesion coating is immersed in a silica sol with a mass concentration of 3% for 10 minutes to obtain a lysozyme phase transition adhesion coating modified with silica, and then the micro-nano structure of silica is filled with silicone oil to obtain a stainless steel material modified with a protein adhesion super-slippery coating.

[0056] Example 8

[0057] 20 mg of L-cysteine ​​was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the pH value was adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution. 200 mg of whey protein was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the two solutions were then mixed evenly to obtain a mixed solution. A silicon wafer was immersed in the mixed solution and cultured at room temperature for 1 hour to form a whey protein phase transition adhesion coating on the surface of the silicon wafer. The whey protein phase transition adhesion coating was then immersed in a silicon carbide dispersion with a mass concentration of 1% (silicon carbide was dispersed in an ethanol aqueous solution with a volume concentration of 60%) for 10 minutes to obtain a lysozyme phase transition adhesion coating modified with silicon carbide. The micro-nano structure of silicon carbide was then filled with corn oil to obtain a silicon wafer modified with a protein adhesion super-slippery coating.

[0058] Example 9

[0059] 50 mg of L-cysteine ​​was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the pH value was adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution; 50 mg of lysozyme was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and then the two solutions were evenly mixed to obtain a mixed solution; a glass sheet was immersed in the mixed solution and cultured at room temperature for 0.5 h to form a lysozyme phase transition adhesion coating on the surface of the glass sheet; then the lysozyme phase transition adhesion coating was immersed in a silica sol with a mass concentration of 3% for 10 minutes to obtain a lysozyme phase transition adhesion coating modified with silica, and then the micro-nano structure of silica was filled with corn oil to obtain a glass sheet modified with a protein adhesion super-slippery coating.

[0060] Depend on Figure 8 It can be seen that the super-slip coating on the glass sheet can resist the adhesion of liquid food (cola, milk, orange juice, coffee, tea, yogurt). Fig. 9 The laser confocal image shows that the super-slippery coating can resist the adhesion of Escherichia coli (there is no fluorescence signal in the laser confocal image). Fig.10 The laser confocal image shows that the super-slip coating can resist the adhesion of Staphylococcus aureus. However, the lysozyme phase change adhesion coating modified directly with corn oil (i.e. without soaking in silica sol) has no anti-adhesion (milk) performance, see Fig.11 .

[0061] Example 10

[0062] 50 mg of L-cysteine ​​was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4 and the pH was adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution. 50 mg of lysozyme was added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and the two solutions were mixed evenly to obtain a mixed solution. The stainless steel sheet was immersed in the mixed solution and cultured at room temperature for 0.5 h to form a lysozyme phase transition adhesion coating on the surface of the stainless steel sheet. The lysozyme phase transition adhesion coating was then immersed in a silica sol with a mass concentration of 3% for 10 min to obtain a lysozyme phase transition adhesion coating modified with silica, and the micro-nano structure of silica was filled with rapeseed oil to obtain a stainless steel sheet modified with a protein adhesion super-slippery coating. Fig.12 It can be seen that the stainless steel sheet modified with the protein adhesion super-slippery coating can resist ice adhesion, while the blank stainless steel sheet is frozen in ice.

[0063] Embodiment 11

[0064] 30 mg of L-cysteine ​​is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4 and the pH is adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution. 30 mg of lysozyme is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH of 7.4, and then the two solutions are mixed evenly to obtain a mixed solution. The mixed solution is sprayed on an iron sheet and incubated at room temperature. After the mixed solution is completely evaporated, a lysozyme phase transition adhesion coating is formed on the surface of the iron sheet. Then, a silica sol with a mass concentration of 3% is sprayed on the lysozyme phase transition adhesion coating. After the solution is evaporated and dried, a lysozyme phase transition adhesion coating modified with silica is obtained. The micro-nano structure of silica is then filled with silicone oil to obtain an iron sheet modified with a protein adhesion super-slippery coating. Fig.13 It can be seen that the iron sheet modified with the protein adhesion super-slippery coating can delay the corrosion of the iron sheet in salt spray.

[0065] Example 12

[0066] 143 mg of tris(2-carboxyethyl)phosphine hydrochloride is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the pH value is adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution; 40 mg of bovine serum albumin is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and then the two solutions are evenly mixed to obtain a mixed solution; the mixed solution is sprayed on a food processing table, incubated at room temperature, and after the mixed solution is completely evaporated to dry, a bovine serum albumin phase transition adhesion coating is formed on the surface of the food processing table; then a silica sol with a mass concentration of 3% is sprayed on the bovine serum albumin phase transition adhesion coating, and after the solution is evaporated to dry, a lysozyme phase transition adhesion coating modified with silica is obtained, and then the micro-nano structure of silica is filled with olive oil to obtain a food processing table modified with a protein adhesion super-slippery coating.

[0067] Example 13

[0068] 40 mg of L-cysteine ​​is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and the pH value is adjusted to 8 with a 5 mol / L sodium hydroxide aqueous solution; 40 mg of lysozyme is added to 10 mL of 4-hydroxyethylpiperazineethanesulfonic acid buffer solution with a pH value of 7.4, and then the two solutions are evenly mixed to obtain a mixed solution; the mixed solution is poured into a milk transport pipeline and immersed, and cultured at room temperature for 1 hour to form a lysozyme phase transition adhesion coating on the inner wall of the milk transport pipeline; then the lysozyme phase transition adhesion coating is immersed in a silica sol with a mass concentration of 3% for 10 minutes to obtain a lysozyme phase transition adhesion coating modified with silica, and then the micro-nano structure of silica is filled with rapeseed oil to obtain a milk transport pipeline modified with a protein adhesion super-slippery coating.

Claims

1. A protein-adhesive super-slip coating, characterized in that: The super-slippery coating is a coating formed by modifying micro-nano particles on a phase transition adhesive coating obtained by reducing proteins with a reducing agent and filling a lubricant, wherein the micro-nano particles have a closely arranged micro-nano structure.

2. The protein adhesion super-slippery coating according to claim 1, characterized in that: The protein includes any one of lysozyme, soy protein, whey protein, lactoferrin, legumin, serum albumin, fibrinogen, zein, collagen, barley protein, gluten, kidney bean protein, keratin, casein, pepsin, myoglobin, lactalbumin, β-lactoglobulin, collagen, albumin, and collagen.

3. The protein-adhesive super-slip coating according to claim 1, characterized in that: The reducing agent includes any one of cysteine, mercaptoethanol, tris(2-carboxyethyl)phosphine hydrochloride, glutathione and dithiothreitol.

4. The protein-adhesive super-slippery coating according to claim 1, characterized in that: The micro-nano particles include any one of silicon dioxide, aluminum oxide, zinc oxide, silicon carbide, silicon nitride, titanium oxide, carbon nanomaterials, and polymer nanoparticles.

5. The protein-adhesive super-slippery coating according to claim 1, characterized in that: The lubricant includes any one of silicone oil, perfluoropolyether, perfluorodecahydronaphthalene, castor oil, coconut oil, corn oil, mustard oil, olive oil, palm oil, rapeseed oil, soybean oil, cottonseed oil and paraffin oil.

6. The protein-adhesive super-slippery coating according to any one of claims 1 to 5, characterized in that The super-slip coating is prepared by any one of the following methods: A 1-100 mg / mL reducing agent 4-hydroxyethylpiperazineethanesulfonic acid buffer solution is adjusted to a pH of 4-10 with NaOH, and then the reducing agent is uniformly mixed with a 1-100 mg / mL protein 4-hydroxyethylpiperazineethanesulfonic acid buffer solution at a volume ratio of 1:1 to obtain a mixed solution; the obtained mixed solution is dip-coated, sprayed or drip-coated on the surface of any material, and cultured at room temperature for 0.1 to 5 hours to modify the protein phase transition adhesion coating on the surface of the material; a micro-nano particle dispersion is dip-coated, sprayed or spin-coated on the protein phase transition adhesion coating to obtain a protein phase transition adhesion coating modified with micro-nano particles; a lubricant is filled in the micro-nano structure of the micro-nano particles to obtain a protein adhesion super-slippery coating.

7. The protein-adhesive super-slippery coating according to claim 6, characterized in that: The pH of a 1-10 mg / mL reducing agent 4-hydroxyethylpiperazineethanesulfonic acid buffer solution is adjusted to 6-9 with NaOH, and then the reducing agent 4-hydroxyethylpiperazineethanesulfonic acid buffer solution and a 1-10 mg / mL protein 4-hydroxyethylpiperazineethanesulfonic acid buffer solution are uniformly mixed at a volume ratio of 1:1 to obtain a mixed solution.

8. The protein-adhesive super-slippery coating according to claim 6, characterized in that: The materials include any one of common experimental materials, materials for food processing equipment, and material transportation pipeline materials, specifically including any one of silicon, glass, quartz, mica, pottery, porcelain, polymethyl methacrylate, polystyrene, polyethylene terephthalate, polycarbonate, polyvinyl chloride, polyvinylidene chloride, polyamide, polyurethane, phenolic resin, rubber, polypropylene, polyethylene, and various alloy materials.

9. Application of the protein adhesion super-slippery coating according to claim 1 in any of the following production and life: (1) Application in the preparation of self-cleaning liquid food transportation pipelines; (2) Application in the preparation of food processing materials that resist microbial and protein adhesion; (3) Application in the preparation of drag-reducing coatings for liquid food transportation pipelines; (4) Application in food processing equipment that resists metal corrosion; (5) Application in the preparation of anti-ice adhesion.

Citation Information

Patent Citations

  • Super sliding ice-proof surface device, and preparation method thereof

    CN108912924A

  • Multifunctional natural super-hydrophobic material and application thereof

    CN112264272A

  • Biomass-based antifouling material and application thereof

    CN115286958A

  • Bionic super-lubricating coating simple and easy to operate and capable of being prepared on large scale and preparation method of bionic super-lubricating coating

    CN115518857A

  • Slippery liquid-infused porous surfaces and biological applications thereof

    US20140187666A1