Low-moisture-permeability type organic silicon sealant and preparation method thereof

By introducing long-chain alkane structure and alkyl modified silicone polymer into the silicone sealant and carrying out hydrophobic treatment of silicate filler, the problem of high vapor transmission rate of silicone sealant in the prior art is solved. The preparation of low moisture permeability sealant is realized, and the stability and economicality of the product are improved.

CN119060686APending Publication Date: 2024-12-03ZHEJIANG XINAN CHEM IND GRP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411317823.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing silicone sealant has insufficient water barrier properties and high water vapor transmission rate, which limits its application in new energy and other fields. In the existing improvement measures, phenyl silicone raw materials are expensive or complex in synthesis, which affects economic benefits. and universality.

Method used

The hydrophobic treatment of silicate filler is performed to increase system compatibility by introducing a hydrophobic structure, including the addition of a solid higher alkane mixture of long-chain alkane structure and a long-chain alkyl modified silicone polymer, and the hydrophobic treatment of silicate filler and increase system compatibility and Hydrophobicity, reducing water vapor transmittance.

Benefits of technology

It realizes the preparation of low moisture permeability silicone sealant, reduces water vapor transmission rate, maintains the strength and bonding performance of the sealant, is suitable for packaging with partial water barrier requirements, and improves the stability and service life of the product. At the same time, it reduces raw material costs and process complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention provides a low moisture permeability type organosilicon sealant and a preparation method thereof. The low moisture permeability type organosilicon sealant comprises alkoxy terminated polydimethylsiloxane / alpha, omega dihydroxy polydimethylsiloxane, silicone oil, an alkyl modified organosilicon polymer, a higher alkane mixture, a reinforcing / semi-reinforcing filler, a silicate filler, a filler treating agent, a cross-linking agent, a silane coupling agent and a catalyst. According to the low-moisture-permeability organosilicon sealant, the silicate filler is subjected to alkyl and fluorosilane modification treatment firstly, then the alkyl modified organosilicon polymer and higher alkane mixture is introduced to prepare the sealant, the low-moisture-permeability organosilicon sealant is obtained, a large amount of long-chain alkane and the filler are mutually cooperated and interspersed, water vapor is prevented from passing through, the water resistance of the sealant is improved, and the water vapor permeability is reduced; the raw materials are cheap, the economic value is high, the water vapor transmission rate is greatly reduced while the necessary strength, elasticity and bonding performance of the organic silicon sealant are maintained, the organic silicon sealant can be applied to packaging with partial water blocking requirements, the stability of a product is improved, and the service life of the product is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of organic silicon, and relates to organic silicon sealant, and in particular to a low moisture permeability organic silicon sealant which can be used in packaging with partial water blocking requirements to improve product stability and service life, and a preparation method thereof. Background Art

[0002] In the future, the new energy industry will continue to develop rapidly. The core batteries, electronic controls, motors, etc. in photovoltaic modules, electric vehicle power batteries, rail transportation, nuclear energy and other industries are easily corroded by water vapor in the air, which reduces their service life. Therefore, they need to be sealed and packaged. Silicone sealant has the advantages of excellent bonding, high weather resistance, good high temperature resistance, good operation and processing performance, and convenient construction. However, its water vapor transmission rate is relatively large (30-50g / m 2 *d), its water vapor barrier performance is very poor, which limits its application in these areas.

[0003] The Chinese patent publication number is CN115044346A, and the publication date is September 13, 2022. The invention patent named "Sealing material and preparation method thereof, solar cell assembly" provides a sealing material, which adds modified olefin polymer and water-absorbing resin to silica gel, which can significantly reduce the water vapor permeability, effectively prevent the edge sealant from being delaminated due to the erosion of hot and humid water vapor by the battery assembly, solve the problem of edge water vapor intrusion and corrosion of the battery cell, and meet the edge sealing packaging requirements very well. However, the modified olefin polymer has low polarity, and has poor compatibility and poor adhesion with the silicone system. The water-absorbing resin affects the deep curing of the sealant in the moisture-curing single-component formula.

[0004] The Chinese patent publication number is CN116376510A, and the publication date is July 4, 2023. The name is a sealant and a preparation method thereof, and an invention patent for a solar cell assembly. The base glue is disclosed, and the base glue includes terminal hydroxyl polydimethylsiloxane and terminal hydroxyl polymethylphenylsiloxane. The sealant has low water permeability and good water blocking effect.

[0005] The Chinese patent publication number is CN117126539A, and the publication date is November 28, 2023. The invention patent is named as a two-component organic silica gel composition with low water permeability. By adding phenyl groups to the single and double components and combining them with sheet silicate fillers, the steric hindrance is increased, thereby achieving the effect of reducing the water vapor transmission rate. However, in the above two patents, the phenyl organic silicone raw materials are expensive, and the presence of benzene steric hindrance also affects the curing activity, and the economic benefits are not high.

[0006] China Patent Publication No. CN116948179A, Publication Date October 27, 2023, Invention Patent Named Modified Cage-type Oligomeric Sisesquioxane, Silicone Sealant and Preparation Method, Flexible Semiconductor Device and Thin Film Encapsulation Method, Using Multifunctional Active Modified Cage-type Oligomeric Sisesquioxane as the Main Component of the Encapsulation Material, and Matching the Corresponding Active Diluent and Photoinitiator to Prepare Silicone Sealant, It Has Low Water Vapor Transmission Rate and High Light Transmittance. However, the synthesis of this complex structure of cage-type silsesquioxane is very difficult, and the silicone sealant is a photocurable type, which is not very versatile. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a low moisture permeability organosilicon sealant and a preparation method thereof. The present invention introduces a hydrophobic structure into each component of the organosilicon sealant formula: 1) a solid high-alkane mixture with a long-chain alkane structure is added in the form of a filler; 2) a long-chain alkyl-modified organosilicon polymer is used to replace part or all of the methyl silicone oil, and a long-chain alkane is introduced into the organosilicon structure to increase the hydrophobicity of the organosilicon, and at the same time, the compatibility of the solid high-alkane mixture with the organosilicon system is improved to avoid precipitation; 3) a long-chain alkyl silane and a fluorosilane are used to pre-treat the filler to increase the compatibility and hydrophobicity of the system, and at the same time, the size between the sheets is increased, so that fillers of different particle sizes are interspersed and coordinated with each other, blocking the circulation of water vapor, improving the hydrophobicity and water-blocking properties of the sealant, and reducing the water vapor transmission rate. The raw materials used in the low moisture permeability organosilicon sealant of the present invention are cheap, the process is relatively universal, and the construction is convenient. It does not affect the strength and bonding properties of the organosilicon sealant itself, and can be used in packaging with partial water-blocking requirements to improve the stability and service life of the product.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] The present invention first provides a low moisture permeability type organic silicone sealant, which comprises, by weight, 25-40 parts of alkoxy-terminated polydimethylsiloxane / α, ω-dihydroxy polydimethylsiloxane, 0-10 parts of silicone oil, 0-20 parts of alkyl-modified organic silicon polymer, 0-30 parts of higher alkane mixture, 10-60 parts of silicic acid filler, 0.1-5 parts of filler treatment agent, 0-50 parts of reinforcing / semi-reinforcing filler, 1-5 parts of crosslinking agent, 0.1-5 parts of silane coupling agent and 0.05-5 parts of catalyst.

[0010] As a preferred embodiment of the present invention, the viscosity of the alkoxy-terminated polydimethylsiloxane at 25°C is 1000-100000 mPa·s, and the alkoxy group includes trimethoxy, triethoxy, methyldimethoxy, vinyldimethoxy, methyldiethoxy or vinyldiethoxy; the viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25°C is 1000-150000 mPa·s.

[0011] As a preferred embodiment of the present invention, the silicone oil is at least one of methyl silicone oil, hydroxy silicone oil, vinyl silicone oil, monohydroxy silicone oil and alkoxy silicone oil with a viscosity of 5-1000 mPa·s.

[0012] As a preferred embodiment of the present invention, the higher alkane mixture is C n H 2n+2 A mixture of higher alkanes composed mainly of n, wherein n is 9-40.

[0013] As a preferred embodiment of the present invention, the layered silicate filler includes one or more of talc, kaolin, wollastonite, feldspar powder, mica powder or montmorillonite, and the reinforcing / semi-reinforcing filler is nano calcium carbonate and fumed silica.

[0014] As a preferred embodiment of the present invention, the filler treating agent is a composition of alkyl silane and fluorosilane.

[0015] As a preferred embodiment of the present invention, the alkylsilane includes one or a combination of octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane or octadecyltriethoxysilane; the fluorosilane includes one or a combination of (3,3,3-trifluoropropyl)dichloromethylsilane, (3,3,3-trifluoropropyl)trichloromethylsilane, 3,3,3-trifluoropropylmethyldimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3,3,3-trifluoropropyltriethoxysilane, tridecafluorooctyltrimethoxysilane, tridecafluorooctyltriethoxysilane, heptadecafluorodecyltrimethoxysilane and heptadecafluorodecyltriethoxysilane.

[0016] As a preferred embodiment of the present invention, the mass ratio of the silicon-based silane to the fluorosilane is 1:10-10:1.

[0017] As a preferred embodiment of the present invention, the crosslinking agent includes one or a combination of methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, propyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, propyltriethoxysilane, phenyltriethoxysilane, tetramethoxysilane or tetraethoxysilane.

[0018] The present invention also provides a method for preparing the above-mentioned low moisture permeability organic silicon sealant, the preparation method comprising the following steps:

[0019] 1) Pretreatment of silicate filler: 10-60 parts of silicate filler to be treated, 0.1-5 parts of silane coupling agent and 5-10 times the weight of deionized water, stir at 70-90°C for 1-2h, filter and dry before use;

[0020] 2) Adding materials: adding alkoxy-terminated polydimethylsiloxane / α, ω dihydroxy polydimethylsiloxane, silicone oil, part of the crosslinking agent, the treated silicate filler obtained in step 1), and the reinforcing / semi-reinforcing filler into a dynamic mixer for heating and mixing; when the temperature is raised to 65° C., adding an alkyl-modified organic silicon polymer and a mixture of higher alkanes, and continuing to heat and mix until the raw materials are completely dissolved;

[0021] 3) Dehydration: The mixture obtained in step 2) is heated to 100°C-120°C and dehydrated by high-speed stirring for 2 hours, and then cooled;

[0022] 4) Glue preparation: lower the temperature to below 50°C, add the remaining cross-linking agent, coupling agent and catalyst, stir for 10-30 minutes and then discharge the material to obtain a low moisture permeability silicone sealant.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1) The silicate filler of the present invention is first subjected to a hydrophobic treatment, which, on the one hand, increases the compatibility and hydrophobicity of the system, and on the other hand, increases the size between the sheets, so that fillers of different particle sizes interpenetrate and cooperate with each other, thereby increasing the water-blocking effect; by adding alkyl-modified silicone polymers and higher alkane mixtures, long-chain alkyl groups are introduced into the silicone structure and formula, thereby further increasing the water-blocking performance and reducing the water vapor permeability.

[0025] 2) The low moisture permeability silicone sealant of the present invention uses cheap and readily available raw materials with high economic value. It reduces water vapor permeability while maintaining the necessary strength, elasticity and bonding properties of the silicone sealant. It can be used in sealing and packaging with partial water-blocking requirements to improve product stability and service life.

[0026] 3) The preparation method of the present invention is simple and the conditions are mild. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0028] The invention provides a low moisture permeability type organic silicone sealant, which comprises, by weight, 25-40 parts of alkoxy-terminated polydimethylsiloxane / α, ω-dihydroxy polydimethylsiloxane, 0-10 parts of silicone oil, 0-20 parts of alkyl-modified organic silicon polymer, 0-30 parts of higher alkane mixture, 10-60 parts of silicic acid filler, 0.1-5 parts of filler treatment agent, 0-50 parts of reinforcing / semi-reinforcing filler, 1-5 parts of crosslinking agent, 0.1-5 parts of silane coupling agent and 0.05-5 parts of catalyst.

[0029] In some embodiments, the viscosity of the alkoxy-terminated polydimethylsiloxane at 25° C. is 1000-100000 mPa·s, specifically 1000 mPa·s, 5000 mPa·s, 10000 mPa·s, 20000 mPa·s, 50000 mPa·s, 80000 mPa·s, 100000 mPa·s, etc.

[0030] In some embodiments, the alkoxy group can be trimethoxy, triethoxy, methyldimethoxy, vinyldimethoxy, methyldiethoxy, vinyldiethoxy, etc., which can be obtained by the condensation reaction of α, ω-dihydroxypolydimethylsiloxane and an alcohol-type crosslinking agent, or by the addition reaction of terminal vinyl silicone oil and hydrogen-containing silane. It can be self-synthesized or commercially available.

[0031] In some embodiments, the viscosity of α,ω-dihydroxypolydimethylsiloxane at 25°C is 1000-500000 mPa·s, specifically 1000 mPa·s, 5000 mPa·s, 10000 mPa·s, 20000 mPa·s, 50000 mPa·s, 80000 mPa·s, 100000 mPa·s, 150000 mPa·s or 500000 mPa·s, etc.

[0032] In some embodiments, the alkoxy-terminated polydimethylsiloxane / α,ω-dihydroxy polydimethylsiloxane is preferably alkoxy-terminated polydimethylsiloxane, and more preferably alkoxy-terminated polydimethylsiloxane obtained by addition reaction of vinyl-terminated silicone oil and hydrogen-containing silane. The product obtained by in-situ mixed condensation reaction of α,ω-dihydroxy polydimethylsiloxane, α,ω-dihydroxy polydimethylsiloxane and alcohol-type crosslinking agent, even if most of Si-OH reacts with the crosslinking agent, will still have some residues, affecting the water barrier properties.

[0033] In some embodiments, the silicone oil is at least one of methyl silicone oil, hydroxy silicone oil, vinyl silicone oil, monohydroxy silicone oil, and alkoxy silicone oil with a viscosity of 5-1000 mPa·s, preferably methyl silicone oil.

[0034] The viscosity may specifically be 5 mPa·s, 10 mPa·s, 50 mPa·s, 100 mPa·s, 150 mPa·s, 200 mPa·s, 250 mPa·s, 300 mPa·s, 350 mPa·s, 500 mPa·s, 800 mPa·s or 1000 mPa·s, more preferably 50 mPa·s, 100 mPa·s or 350 mPa·s.

[0035] In some embodiments, the alkyl-modified organic silicon polymer is prepared by adding hydrogen-containing silicone oil / silicone resin to α-olefin, and can be self-synthesized or directly purchased.

[0036] The preferred one is the product of addition reaction between hydrogenated silicone oil / silicone resin and α-C12 or higher carbon olefins. For example, Shin-Etsu KF-412, Momentive SF1642, 50550 / 8VP, Dow Corning AMS C-30Wax, SW-8005C30 Resin Wax, Siloco 2340, 262-35, 264-38, etc.

[0037] In some embodiments, the higher alkane mixture refers to C n H 2n+2 A mixture of higher alkanes as the main component, wherein n is 9-40, preferably n=14-40, and the commercially available ones may be heavy liquid paraffin or solid paraffin.

[0038] More preferably, n=22-40, such as fully refined paraffin with a melting point above 50°C, such as No. 52, No. 54, No. 56, No. 58, No. 60, No. 62, No. 64. When using solid raw materials, they need to be ground and crushed in advance for easy feeding.

[0039] In some embodiments, the silicate filler is a layered silicate material, including talc, kaolin, wollastonite, feldspar powder, mica powder, montmorillonite, alumina, etc., preferably talc, mica powder, and montmorillonite.

[0040] In some embodiments, the layered silicate material preferably has a talc powder particle size of 1000-8000 mesh, and more preferably has a talc powder particle size of 5000-8000 mesh; preferably, the mica powder has a particle size of 300-5000 mesh, and more preferably, the mica powder has a particle size of 800-2000 mesh. More preferably, the montmorillonite is an organic hydrophobically modified nano-montmorillonite.

[0041] In some embodiments, the ratio of the layered silicate material, preferably talc powder, to mica powder and modified nano-montmorillonite is 10-40:5-15:1-5.

[0042] In some embodiments, the reinforcing / semi-reinforcing filler refers to nano-calcium carbonate and fumed silica, wherein the nano-calcium carbonate refers to nano-calcium carbonate surface-modified with stearic acid, phosphatidic acid or a silane coupling agent; the fumed silica is a hydrophobic fumed silica surface-treated with silane, siloxane or other organic molecules, such as TS-720, TS-530, TS-610 from Cabot Corporation, R805, R812, R972, R974 from Evonik, HDK H15, H20 from Wacker, etc.

[0043] In some embodiments, the filler treating agent is a combination of alkyl silane and fluorosilane, and the addition ratio is between 1:10-:10:1, preferably 2:1-1:2.

[0044] In some embodiments, the alkylsilane in the filler treating agent is preferably a long-chain alkylsilane, including octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane and the like long-chain alkylsilanes, and octadecyltrimethoxysilane and octadecyltriethoxysilane are further preferred.

[0045] In some embodiments, the fluorosilane in the filler treatment agent can be (3,3,3-trifluoropropyl)dichloromethylsilane, (3,3,3-trifluoropropyl)trichloromethylsilane, 3,3,3-trifluoropropylmethyldimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3,3,3-trifluoropropyltriethoxysilane, tridecafluorooctyltrimethoxysilane, tridecafluorooctyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, heptadecafluorodecyltriethoxysilane, etc. Preferred are 3,3,3-trifluoropropylmethyldimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, and 3,3,3-trifluoropropyltriethoxysilane.

[0046] In some embodiments, the crosslinking agent is methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, propyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, propyltriethoxysilane, phenyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, etc., preferably one or more of methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, and further preferably methyltrimethoxysilane, vinyltrimethoxysilane and phenyltrimethoxysilane.

[0047] In some embodiments, the silane coupling agent is γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, β-aminoethyl-γ-aminopropyl trimethoxysilane, β-aminoethyl-γ-aminopropyl triethoxysilane, β-aminoethyl-γ-aminopropyl methyl dimethoxysilane, bis (γ-trimethoxysilyl propyl) amine, γ-glycidyl ether oxypropyl trimethoxysilane, 2- (3,4-epoxycyclohexyl) ethyl trimethoxysilane, 3-isocyanatopropyl triethoxysilane. At least one of alkane, 1,3,5-tris[3-(trimethoxysilyl)propyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 3-aminopropylmethyldimethoxysilane, N-n-butyl-3-aminopropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-anilinopropyltrimethoxysilane, bis-[3-(triethoxysilyl)-propyl]-disulfide, 3-mercaptopropyltrimethoxysilane, and 3-thiocyanatopropyltriethoxysilane.

[0048] In some embodiments, the catalyst is an organic tin or organic titanium, such as dibutyltin dilaurate, dibutyltin diacetate, dibutyldioctyltin, dibutyltin oxide, dimethyltin dineodecanoate, dibutyltin bis(ethyl acetoacetate), dibutyltin bis(acetylacetonate), the reaction product of bis(acetyloxy)dibutyltin and ethyl orthosilicate, tetrabutyl titanate, tetraisopropyl titanate, tetraethyl titanate, diisopropyl bis(acetylacetonate), diisobutyl bis(acetylacetonate), bis(acetylacetonate), bis(ethoxyisopropoxy) titanate, bis(acetylacetonate) (isobutoxyisopropoxy) titanate, diisobutyl bis(ethyl acetoacetate), bis(alkoxy)titanium, etc., or a mixture thereof.

[0049] In various embodiments of the present invention, the method for preparing the low moisture permeability organic silicone sealant comprises:

[0050] 1) Pretreatment of silicate fillers (talcum powder and mica powder): 10-60 parts of fillers, 0.1-5 parts of long-chain alkyl silane and fluorosilane, and 5-10 times the weight of deionized water are stirred at 70-90°C for 1-2 hours, filtered and dried for use; long-chain alkyl groups and fluorine-containing groups are used to cover the surface or interlayer of the filler, making it hydrophilic to hydrophobic, while increasing the interlayer spacing, improving the adsorption and dispersibility, and the synergistic interpenetration of different fillers, blocking the flow of water vapor;

[0051] 2) Feeding: Add alkoxy-terminated polydimethylsiloxane / α, ω dihydroxy polydimethylsiloxane, silicone oil, part of the crosslinking agent, treated silicate, and reinforcing / semi-reinforcing filler into a dynamic mixer for heating and mixing; when the temperature reaches 65°C, add the alkyl-modified polymer and the higher alkane mixture, continue to heat and slowly mix until the raw materials are completely dissolved;

[0052] 3) Dehydration: The mixture is heated to 100°C-120°C and dehydrated by high-speed stirring for 2 hours, and then cooled;

[0053] 4) Glue preparation: lower the temperature to below 50°C, add the remaining cross-linking agent, coupling agent and catalyst, stir for 10-30 minutes and then discharge the material to obtain a low moisture permeability silicone material.

[0054] Example 1

[0055] This embodiment provides a method for preparing a low moisture permeability organic silicone sealant, comprising:

[0056] 1) Pretreatment of silicate filler: 30 parts of 5000 mesh talc powder, 10 parts of 1250 mesh mica powder, 1 part of octadecyltrimethoxysilane, 1 part of 3,3,3-trifluoropropyltrimethoxysilane, and 250 parts of deionized water are stirred at 70-90°C for 1-2 hours, and then filtered and dried for use.

[0057] 2) Adding materials: adding 30 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 100,000 mPa.s, 2 parts of 50 mPa.s methyl silicone oil, 2 parts of methyltrimethoxysilane crosslinking agent, talc powder and mica powder treated in step 1), 1 part of hydrophobic silica Wacker H20, and 4 parts of nano-organic modified montmorillonite into a dynamic mixer for heating and mixing; when the temperature is raised to 65° C., adding 15 parts of alkyl-modified polymer KF-412 and 10 parts of No. 58 paraffin wax, continuing to heat and slowly mixing until the raw materials are completely dissolved.

[0058] 3) Dehydration: Heat the mixture to 100°C-120°C and dehydrate with high-speed stirring for 2 hours, then cool down.

[0059] 4) Glue preparation: lower the temperature to below 50° C., add 2 parts of methyltrimethoxysilane, 0.4 parts of KH560 and 1.8 parts of bis(acetylacetonato)(isobutoxyisopropoxy)titanate, stir for 10-30 minutes and then discharge the material to obtain a low moisture permeability silicone sealant 1.

[0060] Example 2

[0061] This embodiment provides a method for preparing a low moisture permeability organic silicone sealant, comprising:

[0062] 1) Pretreatment of silicate filler: 40 parts of 5000 mesh talc powder, 15 parts of 1250 mesh mica powder, 1.5 parts of octadecyltrimethoxysilane, 0.8 parts of 3,3,3-trifluoropropyltrimethoxysilane, and 300 parts of deionized water are stirred at 70-90°C for 1-2 hours, and then filtered and dried for use.

[0063] 2) Adding materials: adding 28 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 100,000 mPa.s, 4 parts of 50 mPa.s methyl silicone oil, 2 parts of methyltrimethoxysilane crosslinking agent, talc powder and mica powder treated in step 1), 2 parts of Wacker H20, and 2 parts of nano-organic modified montmorillonite into a dynamic mixer for heating and mixing; when the temperature is raised to 65° C., adding 10 parts of alkyl-modified polymer KF-412 and 20 parts of No. 62 paraffin wax, continuing to heat and slowly mixing until the raw materials are completely dissolved.

[0064] 3) Dehydration: Heat the mixture to 100°C-120°C and dehydrate with high-speed stirring for 2 hours, then cool down.

[0065] 4) Glue preparation: lower the temperature to below 50°C, add 1.5 parts of methyltrimethoxysilane, 0.5 parts of phenyltrimethoxysilane, 0.4 parts of KH560 and 1.8 parts of diisobutyl bis(ethyl acetoacetate) titanate, stir for 10-30 minutes and then discharge to obtain low moisture permeability silicone sealant 2.

[0066] Example 3

[0067] This embodiment provides a method for preparing a low moisture permeability organic silicone sealant, comprising:

[0068] 1) Pretreatment of silicate filler: 30 parts of 8000 mesh talc powder, 10 parts of 800 mesh mica powder, 1 part of octadecyl triethoxysilane, 1.5 parts of 3,3,3-trifluoropropyl triethoxysilane and 280 parts of deionized water are stirred at 70-90°C for 1-2 hours, filtered and dried for use.

[0069] 2) Adding materials: 30 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 40,000 mPa.s, 2 parts of methyltrimethoxysilane crosslinking agent, talc powder and mica powder treated in step 1), 3 parts of white carbon Wacker H20, and 3 parts of nano-organic modified montmorillonite are added to a dynamic mixer for heating and mixing; when the temperature is raised to 65°C, 15 parts of alkyl-modified polymer SF1642 and 15 parts of No. 62 paraffin are added, and the temperature is continued to be raised and slowly mixed until the raw materials are completely dissolved.

[0070] 3) Dehydration: Heat the mixture to 100°C-120°C and dehydrate with high-speed stirring for 2 hours, then cool down.

[0071] 4) Glue preparation: lower the temperature to below 50°C, add 1.5 parts of methyltrimethoxysilane, 0.5 parts of vinyltrimethoxysilane, 0.5 parts of KH560 and 1.8 parts of diisobutyl bis(ethyl acetoacetate)titanate, stir for 10-30 minutes and then discharge to obtain low moisture permeability organic silicone sealant 3.

[0072] Example 4

[0073] This embodiment provides a method for preparing a low moisture permeability organic silicone sealant, comprising:

[0074] 1) Pretreatment of silicate filler: 10 parts of 5000 mesh talc powder, 30 parts of 1250 mesh mica powder, 0.8 parts of octadecyltrimethoxysilane, 0.8 parts of 3,3,3-trifluoropropylmethyldimethoxysilane, and 100 parts of deionized water are stirred at 70-90°C for 1-2 hours, filtered and dried for use.

[0075] 2) Adding materials: 30 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 50,000 mPa.s, 2 parts of methyltrimethoxysilane crosslinking agent, talcum powder and mica powder treated in step 1), and 35 parts of nano-calcium are added to a dynamic mixer for heating and mixing; when the temperature is raised to 65°C, 20 parts of alkyl-modified silicone polymer SF1642 are added, and the temperature is continued to be raised and slowly mixed until the raw materials are completely dissolved.

[0076] 3) Dehydration: Heat the mixture to 100°C-120°C and dehydrate with high-speed stirring for 2 hours, then cool down.

[0077] 4) Glue preparation: lower the temperature to below 50°C, add 1.5 parts of methyltrimethoxysilane, 0.5 parts of phenyltrimethoxysilane, 0.4 parts of KH560 and 1.8 parts of diisobutyl bis(ethyl acetoacetate) titanate, stir for 10-30 minutes and then discharge to obtain low moisture permeability silicone sealant 4.

[0078] Example 5

[0079] This embodiment provides a method for preparing a low moisture permeability organic silicone sealant, comprising:

[0080] 1) Pretreatment of silicate filler: 30 parts of 5000 mesh talc powder, 10 parts of 600 mesh mica powder, 1.5 parts of octadecyltrimethoxysilane, 1 part of 3,3,3-trifluoropropylmethyldimethoxysilane and 250 parts of deionized water are stirred at 70-90°C for 1-2 hours, and then filtered and dried for use.

[0081] 2) Adding materials: 35 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 50,000 mPa.s, 2 parts of methyltrimethoxysilane crosslinker, talcum powder and mica powder treated in step 1), and 3 parts of Wacker H20 are added to a dynamic mixer for heating and mixing; when the temperature is raised to 65°C, 15 parts of No. 52 paraffin are added, and the temperature is continued to be raised and slowly mixed until the raw materials are completely dissolved.

[0082] 3) Dehydration: Heat the mixture to 100°C-120°C and dehydrate with high-speed stirring for 2 hours, then cool down.

[0083] 4) Glue preparation: lower the temperature to below 50°C, add 1.5 parts of methyltrimethoxysilane, 0.5 parts of phenyltrimethoxysilane, 0.4 parts of KH560 and 1.8 parts of diisobutyl bis(ethyl acetoacetate)titanate, stir for 10-30 minutes and then discharge the material to obtain low moisture permeability silicone sealant 5.

[0084] Comparative Example 1

[0085] 30 parts of trimethoxy-terminated polydimethylsiloxane with a viscosity of 50,000 mPa.s, 1.5 parts of methyltrimethoxysilane, and 0.5 parts of phenyltrimethoxysilane crosslinking agent were added into a blender and mixed evenly. Then, 0.4 parts of KH560 and 1.8 parts of diisobutyl bis(ethyl acetoacetate) titanate were added and stirred for 10-30 minutes before discharging to obtain silicone sealant 6.

[0086] Comparative Example 2

[0087] The alkyl-modified organic silicon polymer in Example 1 was replaced with 350 mPa·s methyl silicone oil, and the talc powder, the higher alkane mixture, the mica powder and the montmorillonite were all replaced with nano-calcium carbonate, while other conditions remained unchanged, to obtain organic silicon sealant 7.

[0088] Comparative Example 3

[0089] The alkyl-modified organic silicon polymer in Example 1 was replaced with 350 mPa·s methyl silicone oil, and the talc powder, the higher alkane mixture, the mica powder and the montmorillonite were all replaced with 5000 mesh talc powder, while other factors remained unchanged, to obtain organic silicon sealant 8.

[0090] Comparative Example 4

[0091] The alkyl-modified organic silicon polymer in Example 2 was replaced with 350 mPa·s methyl silicone oil, talc powder, mica powder and montmorillonite were all replaced with nano-calcium carbonate, and the higher alkane mixture was changed to 10 parts, to obtain organic silicon sealant 9.

[0092] Comparative Example 5

[0093] The alkyl-modified organic silicon polymer in Example 2 was replaced with 350 mPa·s methyl silicone oil, talc powder, mica powder and montmorillonite were all replaced with nano-calcium carbonate, and the filler pretreatment was removed. Others remained unchanged to obtain an organic silicon sealant 10.

[0094] Comparative Example 6

[0095] The higher alkane mixture, talcum powder, mica powder and montmorillonite in Example 3 were all replaced with nano-calcium, and the other components remained unchanged to obtain an organosilicon sealant 11.

[0096] Comparative Example 7

[0097] The pre-treatment of the silicate filler in Example 4 was removed, and the rest remained unchanged to obtain an organosilicon sealant 12.

[0098] The organosilicon sealants obtained in Examples 1-5 and the organosilicon sealants obtained in Comparative Examples 1-7 were tested. The test results are shown in Table 1.

[0099] Water vapor transmission rate and moisture permeability coefficient test: According to ASTM F1249, the test was carried out on a C391F water vapor transmission rate tester. The experimental conditions were temperature 23°C, humidity 50%, and test area 50cm 2 , the sample thickness is 1mm.

[0100] Hardness test:

[0101] Tensile strength test: GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber" is used to test the tensile strength and elongation of the sealant.

[0102] Adhesion test: According to method B (hand pull test) in Appendix D of GB / T 16776-2005, the substrates are glass, anodized aluminum and stainless steel for adhesion test. Complete cohesive failure is 5, and complete peeling is 0.

[0103] Extrusion test: Referring to GB / T 13477.4-2017, the plastic nozzle used was cut into an inner diameter of 4 mm, and the air pressure was adjusted to 300 kPa.

[0104] Table 1. Test results

[0105]

[0106]

[0107] See Table 1. The water vapor transmission rate of silicone without filler is 40g / m 2 *24h (Comparative Example 1), the water vapor transmission rate of the conventional alcohol-mixed formula with calcium carbonate as filler is 20g / m 2 * More than 24h (Comparative Example 2), the water vapor transmission rate of the low moisture permeability silicone sealant of the present invention can reach 3g / m 2 * Below 24h, it can be seen from Comparative Examples 3, 4 and 6 that the use of silicate fillers or alkyl-modified silicone polymers or higher alkane mixtures alone can also partially reduce the water vapor transmission rate. In Comparative Example 5, when the filler is not treated with silane and no alkyl-modified silicone polymer is added, precipitation occurs when 20 parts of paraffin is added. In Comparative Example 7, after the pre-treatment of the filler is removed, the dispersibility of the entire system is affected, the colloid is too thick, and the extrusion is 3, which cannot be used.

[0108] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A low moisture permeability silicone sealant, characterized in that: The low moisture permeability organic silicone sealant comprises, by weight, 25-40 parts of alkoxy-terminated polydimethylsiloxane / α,ω-dihydroxy polydimethylsiloxane, 0-10 parts of silicone oil, 0-20 parts of alkyl-modified organic silicone polymer, 0-30 parts of higher alkane mixture, 10-60 parts of silicic acid filler, 0.1-5 parts of filler treatment agent, 0-50 parts of reinforcing / semi-reinforcing filler, 1-5 parts of crosslinking agent, 0.1-5 parts of silane coupling agent and 0.05-5 parts of catalyst.

2. A low moisture permeability organic silicone sealant according to claim 1, characterized in that: The viscosity of the alkoxy-terminated polydimethylsiloxane at 25° C. is 1000-100000 mPa·s, and the alkoxy group includes trimethoxy, triethoxy, methyldimethoxy, vinyldimethoxy, methyldiethoxy or vinyldiethoxy; the viscosity of the α,ω-dihydroxy polydimethylsiloxane at 25° C. is 1000-150000 mPa·s.

3. The low moisture permeability organic silicone sealant according to claim 1, characterized in that: The silicone oil is at least one of methyl silicone oil, hydroxy silicone oil, vinyl silicone oil, monohydroxy silicone oil and alkoxy silicone oil with a viscosity of 5-1000 mPa·s.

4. The low moisture permeability organic silicone sealant according to claim 1, characterized in that: The higher alkane mixture is C n H 2n+2 A mixture of higher alkanes composed mainly of n, wherein n is 9-40.

5. The low moisture permeability organic silicone sealant according to claim 1, characterized in that: The layered silicate filler includes one or more of talc, kaolin, wollastonite, feldspar powder, mica powder or montmorillonite, and the reinforcing / semi-reinforcing filler is nano calcium carbonate and fumed silica.

6. The low moisture permeability organic silicone sealant according to claim 1, characterized in that: The filler treating agent is a composition of alkyl silane and fluorosilane.

7. The low moisture permeability organic silicone sealant according to claim 6, characterized in that: The alkylsilane includes one or a combination of octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane or octadecyltriethoxysilane; the fluorosilane includes one or a combination of (3,3,3-trifluoropropyl)dichloromethylsilane, (3,3,3-trifluoropropyl)trichloromethylsilane, 3,3,3-trifluoropropylmethyldimethoxysilane, 3,3,3-trifluoropropyltrimethoxysilane, 3,3,3-trifluoropropyltriethoxysilane, tridecafluorooctyltrimethoxysilane, tridecafluorooctyltriethoxysilane, heptadecafluorodecyltrimethoxysilane and heptadecafluorodecyltriethoxysilane.

8. The low moisture permeability organic silicone sealant according to claim 6, characterized in that: The mass ratio of the silicon-based silane to the fluorosilane is 1:10-10:

1.

9. The low moisture permeability organic silicone sealant according to claim 1, characterized in that: The crosslinking agent includes one or a combination of methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, propyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, propyltriethoxysilane, phenyltriethoxysilane, tetramethoxysilane or tetraethoxysilane.

10. A method for preparing a low moisture permeability organic silicone sealant according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: 1) Pretreatment of silicate filler: 10-60 parts of silicate filler to be treated, 0.1-5 parts of silane coupling agent and 5-10 times the weight of deionized water, stir at 70-90°C for 1-2h, filter and dry before use; 2) Adding materials: adding alkoxy-terminated polydimethylsiloxane / α, ω dihydroxy polydimethylsiloxane, silicone oil, part of the crosslinking agent, the treated silicate filler obtained in step 1), and the reinforcing / semi-reinforcing filler into a dynamic mixer for heating and mixing; when the temperature is raised to 65° C., adding an alkyl-modified organic silicon polymer and a mixture of higher alkanes, and continuing to heat and mix until the raw materials are completely dissolved; 3) Dehydration: The mixture obtained in step 2) is heated to 100°C-120°C and dehydrated by high-speed stirring for 2 hours, and then cooled; 4) Glue preparation: lower the temperature to below 50°C, add the remaining cross-linking agent, coupling agent and catalyst, stir for 10-30 minutes and then discharge the material to obtain a low moisture permeability silicone sealant.

Citation Information

Cited By