Preparation method of high-temperature phase change heat storage ball
By adding high-melting point elastic material to the phase change material of aluminum-silicon alloy and encapsulating it with a core structure, the corrosion resistance of stainless steel shells is enhanced by hot-dip plating and micro-arc oxidation technology, the phase change heat storage material of aluminum-silicon alloy is solved. Oxidation and leakage problems improve their mechanical strength and heat storage capacity, and achieve efficient high-temperature phase change heat storage effect.
Patent Information
- Application Number
- CN202411171515.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The phase change heat storage material of aluminum-silicon alloy is prone to oxidation during the phase change process, has strong corrosiveness, and the phase change medium is prone to leakage, resulting in poor packaging effect, low mechanical strength, and insufficient heat storage per unit volume, which affects its practical application.
High-energy ball mill equipment is used to mix aluminum-silicon alloy phase change materials and high melting point elastic materials to prepare stainless steel heat storage ball shells and generate dense alumina layer through hot dip plating and micro-arc oxidation technology to form a shell structure to improve corrosion resistance and machinery Strength to prevent stress and leakage caused by volume changes.
The packaging effect, leakage resistance, heat storage per unit volume and mass, mechanical strength and service life of aluminum-silicon alloy phase change heat storage balls are significantly improved, ensuring thermal cycle stability and high-temperature application capabilities.
Smart Images

Figure CN119060694A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature phase-change heat storage, and specifically to a method for preparing a high-temperature phase-change heat storage ball. Background Art
[0002] Energy is the key to the development of human society. Energy resources are a prerequisite for the development of industries such as industry, agriculture, communications and information technology in any society. my country will vigorously develop and utilize new energy sources such as solar energy, and improving energy utilization efficiency will be the development trend in the energy field. Solar energy and industrial waste heat have the disadvantages of discontinuity and instability. Heat storage technology can match energy supply and demand in time, space and intensity. Heat storage technology includes three categories: sensible heat storage, latent heat storage (also known as phase change storage) and chemical reaction heat storage. Among them, phase change heat storage technology is to store and release heat energy through the solid-liquid phase change process of phase change material (PCM). It has the advantages of high heat storage density, stable phase change temperature and easy process control. It can store a large amount of heat under a small temperature difference and is an effective heat storage method. High-temperature phase change heat storage in the three temperature zones of low temperature, medium temperature and high temperature of phase change heat storage has the characteristics of high thermal energy quality, high heat storage density, and approximately isothermal heat storage and heat release processes. It has significant advantages in industrial waste heat recovery, solar thermal power generation and power peak shifting and valley filling.
[0003] Phase change material (PCM) is the key core of phase change thermal storage technology. As a metal-based phase change thermal storage material, the main characteristics of aluminum silicon alloy include: high thermal storage density (latent heat of 400-500 kJ / kg): aluminum silicon alloy has a high thermal storage density and can store a large amount of heat in a relatively small volume. Stable phase change temperature: The phase change temperature of aluminum silicon alloy can be controlled by adjusting the ratio of aluminum and silicon, so that it can achieve efficient heat exchange within the required temperature range. Good cycle stability: aluminum silicon alloy shows good stability during multiple phase change cycles, ensuring its reliability in long-term use. In addition, silicon and aluminum elements are widely available and have low cost. However, aluminum silicon alloy phase change thermal storage materials are easily oxidized during the phase change process, are highly corrosive, the phase change medium is easy to leak, and the volume changes from solid to liquid, which limits the practical application of aluminum silicon alloy phase change thermal storage materials. One of the main ways to solve the above problems is to encapsulate aluminum silicon alloy.
[0004] In recent years, some scholars have conducted extensive research on the packaging of aluminum-silicon alloys. For example, the patented technology of "A method for preparing an aluminum-based metal phase-change heat storage capsule" (CN118344849A) is as follows: 1. Place aluminum-based metal powder in a spheroidizing machine and prepare the aluminum-based metal powder into a spherical core with the help of a binder; 2. Use a coating drum device to coat the spherical core with a certain thickness of an inorganic ceramic powder shell; 3. After molding, drying, low-temperature pre-sintering, and high-temperature sintering, a large phase-change heat storage capsule with an inorganic ceramic shell coated with aluminum-based metal is obtained. The method is simple and environmentally friendly, but the mechanical strength of the heat storage capsules is relatively weak, and the heat storage per unit volume is low; the patented technology of "a composite material phase change heat storage ball and its preparation method" (CN107988506A) is as follows: 1. Place aluminum silicon alloy powder in a ball forming machine, and intermittently spray aluminum dihydrogen phosphate solution to prepare aluminum silicon alloy balls; 2. Spray a surface modifier on the aluminum silicon alloy balls, and then add α-Al in the ball forming machine. 2 O 3 The powder is rolled into a ball to obtain a composite material phase change thermal storage ball blank; third, deionized water is sprayed on the composite material phase change thermal storage ball blank, and α-Al is added after 10 to 30 seconds. 2 O 3 Powder, rolling, to obtain composite material phase change thermal storage ball blank Ⅰ; repeat the preparation process of composite material phase change thermal storage ball blank Ⅰ until the diameter ratio of composite material phase change thermal storage ball blank n to the diameter of the aluminum silicon alloy ball is 6: (1-5). The composite material phase change thermal storage ball blank n is placed in a muffle furnace, kept at 800-1500℃ for 2-8h, to obtain a composite material phase change thermal storage ball. The invention has simple process and low cost, and has good packaging effect, but it is easy to cause the oxide shell to rupture during the heating process, affecting the energy storage effect. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art and provide a method for preparing a high-temperature phase-change thermal storage ball. The high-temperature phase-change thermal storage ball prepared by the method has good packaging effect on aluminum-silicon alloy, significant anti-leakage effect, high heat storage capacity per unit volume and unit mass, high mechanical strength, high operating temperature, good thermal cycle stability and long service life.
[0006] To achieve the above object, a technical solution adopted by the present invention is:
[0007] Step 1: Pre-treat the raw materials to ensure that all raw materials are dry and purified to prevent contamination or reaction during the mixing process; use high-energy ball mill equipment to mix, place aluminum-silicon alloy phase change material powder and high melting point elastic material powder in a container at 30-50°C, and use high-speed rotating balls or rods to accelerate the mixing process, which lasts for 5-10 minutes. Mechanical mixing can ensure that the materials are fully and evenly mixed together to obtain the required "core" material.
[0008] Step 2: Prepare a stainless steel thermal storage spherical shell. First, use hot-dip plating technology to plate aluminum on the stainless steel surface. Then, based on micro-arc processing technology, a dense and uniform aluminum oxide layer is generated on the stainless steel metal surface through an electrochemical process to improve the corrosion resistance of the shell to molten aluminum-silicon alloy. The prepared stainless steel thermal storage spherical shell can maintain stability and long-term durability in a complex working environment, providing reliable protection and support for the storage and application of molten aluminum-silicon alloy.
[0009] Step 3: Fill the evenly mixed "core" material obtained in step 1 into the stainless steel heat storage ball shell obtained in step 2 to obtain a high-temperature phase change heat storage ball with a "shell-core" structure.
[0010] The aluminum-silicon alloy phase change material is an aluminum-silicon alloy powder with a silicon content of 7 to 20 wt% and a powder particle size of 50 to 150 um. ;
[0011] The high melting point elastic material is aluminum oxide (Al 2 O 3 ) reinforced composite materials or silicon nitride (Si 3 N 4 ) reinforced composite materials, etc., provide a certain elastic deformation, and reduce the stress caused by volume change in the phase change process of aluminum silicon alloy; the powder particle size is 20~200um.
[0012] The mass ratio of the aluminum-silicon alloy phase change material powder to the high melting point elastic material powder is 1:0.1-0.3.
[0013] The stainless steel material is 300 series stainless steel such as 304 stainless steel (06Cr19Ni10), 310 stainless steel (20Cr25Ni20) and 316 stainless steel (06Cr17Ni12Mo2).
[0014] The aluminum layer is plated on the stainless steel metal by hot-dip plating process, the temperature of the hot-dip aluminum plating liquid is 750° C., and the hot-dip plating time is 10 to 20 minutes.
[0015] The hot-dip aluminum-plated stainless steel metal is placed in the electrolyte of the micro-arc oxidation device, the aluminum-plated stainless steel is used as the anode, and the stainless steel conductor is used as the cathode; the process parameters during the oxidation process are: the current density is controlled at 10-20A / dm2 , the oxidation time is 30 to 70 minutes, and the electrolyte temperature is not higher than 60°C.
[0016] In summary, the present invention has the following beneficial effects:
[0017] The core material of the high-temperature phase-change heat storage ball prepared by the present invention is aluminum-silicon alloy, which is cheap and easy to obtain, and has low cost. The main material of the shell material is 300 series stainless steel such as 304 stainless steel (06Cr19Ni10), 310 stainless steel (20Cr25Ni20) and 316 stainless steel (06Cr17Ni12Mo2), etc., which has high mechanical strength and high compressive strength.
[0018] The present invention mixes high melting point elastic material powder with aluminum silicon alloy phase change material powder to provide a certain elastic deformation, thereby reducing the stress generated by volume change of the aluminum silicon alloy phase change material during the high-temperature phase change process, and ensuring that the heat storage ball will not be damaged due to volume change during the high-temperature phase change process, resulting in leakage of the phase change medium.
[0019] The present invention utilizes micro-arc processing technology to generate a dense and uniform aluminum oxide layer on the surface of stainless steel metal through an electrochemical process, thereby improving the corrosion resistance of the shell to molten aluminum-silicon alloy; the prepared stainless steel thermal storage spherical shell can maintain stability and long-term durability in a complex working environment, providing reliable protection and support for the storage and application of molten aluminum-silicon alloy.
[0020] The macroscopic installation method of the core-shell structure adopted in the present invention can greatly increase the specific gravity of the core material in the core-shell ratio, while isolating the contact between the core material aluminum-silicon alloy and oxygen, providing an oxygen-free environment for the core material to carry out the heat storage and release cycle process, effectively exerting the heat storage performance of the core material aluminum-silicon alloy and ensuring its cyclic stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The present invention is a flow chart of the method for preparing the high-temperature phase-change thermal storage ball.
[0022] Figure 2 This is a schematic structural diagram of the high-temperature phase-change heat storage ball of the present invention, in which 1 represents high melting point elastic material powder, 2 represents a stainless steel shell layer, 3 represents a dense alumina coating layer, and 4 represents an aluminum silicon alloy. DETAILED DESCRIPTION
[0023] The specific embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings to facilitate a better understanding and implementation of the present invention. However, it should be emphasized that the present invention is not limited to the following specific embodiments, and can be appropriately adjusted and modified according to actual needs.
[0024] The present invention provides a method for preparing a high-temperature phase-change heat storage ball. Figure 2 As shown, the high-temperature phase-change heat storage ball is a sphere with a diameter of 70 to 150 mm, and the structure is a stainless steel outer shell and an alumina coating that constitute the shell, and an aluminum silicon alloy powder and a high melting point elastic material powder that constitute the "core". The stainless steel outer shell is 2 to 5 mm thick, the alumina coating is 3 to 4 mm thick, the diameter of the "core" is 60 to 140 mm, and the volume of the "core" accounts for more than 70% of the volume of the heat storage ball, ensuring the heat storage capacity of the heat storage ball.
[0025] Example 1
[0026] The invention discloses a method for preparing a high-temperature phase-change heat storage ball.
[0027] Step 1: Pre-treat the raw materials to ensure that all raw materials are dry and purified to prevent contamination or reaction during the mixing process; use high-energy ball mill equipment to mix, place aluminum-silicon alloy phase change material powder and high melting point elastic material powder in a container at 30-50°C, and use high-speed rotating balls or rods to accelerate the mixing process, which lasts for 5-10 minutes. Mechanical mixing can ensure that the materials are fully and evenly mixed together to obtain the required "core" material.
[0028] Step 2: Prepare a stainless steel thermal storage spherical shell. First, use hot-dip plating technology to plate aluminum on the stainless steel surface. Then, based on micro-arc processing technology, a dense and uniform aluminum oxide layer is generated on the stainless steel metal surface through an electrochemical process to improve the corrosion resistance of the shell to molten aluminum-silicon alloy. The prepared stainless steel thermal storage spherical shell can maintain stability and long-term durability in a complex working environment, providing reliable protection and support for the storage and application of molten aluminum-silicon alloy.
[0029] Step 3: Fill the evenly mixed "core" material obtained in step 1 into the stainless steel heat storage ball shell obtained in step 2 to obtain a high-temperature phase change heat storage ball with a "shell-core" structure.
[0030] The aluminum-silicon alloy phase change material is an aluminum-silicon alloy powder with a silicon content of 7 to 12 wt%, and a powder particle size of 50 to 80 um.
[0031] The high melting point elastic material is aluminum oxide (Al 2 O 3 ) reinforced composite materials, provide a certain elastic deformation, and reduce the stress caused by volume change in the phase change process of aluminum-silicon alloy; the powder particle size is 20 to 100 um.
[0032] The mass ratio of the aluminum-silicon alloy phase change material powder to the high melting point elastic material powder is 1:0.1.
[0033] The stainless steel material is 304 stainless steel (06Cr19Ni10).
[0034] The aluminum layer is plated on the stainless steel metal by hot-dip plating process, the temperature of the hot-dip aluminum plating liquid is 750° C., and the hot-dip plating time is 15 to 20 minutes.
[0035] The hot-dip aluminum-plated stainless steel metal is placed in the electrolyte of the micro-arc oxidation device, the aluminum-plated stainless steel is used as the anode, and the stainless steel conductor is used as the cathode; the process parameters during the oxidation process are: the current density is controlled at 10A / dm 2 , the oxidation time is 70 minutes and the electrolyte temperature is not higher than 60℃.
[0036] Example 2
[0037] The invention discloses a method for preparing a high-temperature phase-change heat storage ball.
[0038] Step 1: Pre-treat the raw materials to ensure that all raw materials are dry and purified to prevent contamination or reaction during the mixing process; use high-energy ball mill equipment to mix, place aluminum-silicon alloy phase change material powder and high melting point elastic material powder in a container at 30-50°C, and use high-speed rotating balls or rods to accelerate the mixing process, which lasts for 5-10 minutes. Mechanical mixing can ensure that the materials are fully and evenly mixed together to obtain the required "core" material.
[0039] Step 2: Prepare a stainless steel thermal storage spherical shell. First, use hot-dip plating technology to plate aluminum on the stainless steel surface. Then, based on micro-arc processing technology, a dense and uniform aluminum oxide layer is generated on the stainless steel metal surface through an electrochemical process to improve the corrosion resistance of the shell to molten aluminum-silicon alloy. The prepared stainless steel thermal storage spherical shell can maintain stability and long-term durability in a complex working environment, providing reliable protection and support for the storage and application of molten aluminum-silicon alloy.
[0040] Step 3: Fill the evenly mixed "core" material obtained in step 1 into the stainless steel heat storage ball shell obtained in step 2 to obtain a high-temperature phase change heat storage ball with a "shell-core" structure.
[0041] The aluminum-silicon alloy phase change material is an aluminum-silicon alloy powder with a silicon content of 12 wt % and a powder particle size of 80 to 120 um.
[0042] The high melting point elastic material is aluminum oxide (Al 2 O 3 ) reinforced composite materials, provide a certain elastic deformation, and reduce the stress caused by volume change in the phase change process of aluminum-silicon alloy; the powder particle size is 100-150um.
[0043] The mass ratio of the aluminum-silicon alloy phase change material powder to the high melting point elastic material powder is 1:0.2.
[0044] The stainless steel material is 310 stainless steel (20Cr25Ni20).
[0045] The aluminum layer is plated on the stainless steel metal by hot-dip plating process, the temperature of the hot-dip aluminum plating liquid is 750° C., and the hot-dip plating time is 15 to 20 minutes.
[0046] The hot-dip aluminum-plated stainless steel metal is placed in the electrolyte of the micro-arc oxidation device, the aluminum-plated stainless steel is used as the anode, and the stainless steel conductor is used as the cathode; the process parameters during the oxidation process are: the current density is controlled at 15A / dm 2 , the oxidation time is 50 minutes and the electrolyte temperature is not higher than 60℃.
[0047] Example 3
[0048] The invention discloses a method for preparing a high-temperature phase-change heat storage ball.
[0049] Step 1: Pre-treat the raw materials to ensure that all raw materials are dry and purified to prevent contamination or reaction during the mixing process; use high-energy ball mill equipment to mix, place aluminum-silicon alloy phase change material powder and high melting point elastic material powder in a container at 30-50°C, and use high-speed rotating balls or rods to accelerate the mixing process, which lasts for 5-10 minutes. Mechanical mixing can ensure that the materials are fully and evenly mixed together to obtain the required "core" material.
[0050] Step 2: Prepare a stainless steel thermal storage spherical shell. First, use hot-dip plating technology to plate aluminum on the stainless steel surface. Then, based on micro-arc processing technology, a dense and uniform aluminum oxide layer is generated on the stainless steel metal surface through an electrochemical process to improve the corrosion resistance of the shell to molten aluminum-silicon alloy. The prepared stainless steel thermal storage spherical shell can maintain stability and long-term durability in a complex working environment, providing reliable protection and support for the storage and application of molten aluminum-silicon alloy.
[0051] Step 3: Fill the evenly mixed "core" material obtained in step 1 into the stainless steel heat storage ball shell obtained in step 2 to obtain a high-temperature phase change heat storage ball with a "shell-core" structure.
[0052] The aluminum-silicon alloy phase-change material is an aluminum-silicon alloy powder with a silicon content of 12-20 wt % and a powder particle size of 120-150 um.
[0053] The high melting point elastic material is silicon nitride (Si 3 N 4 ) reinforced composite materials, provide a certain elastic deformation, and reduce the stress caused by volume change in the phase change process of aluminum-silicon alloy; the powder particle size is 150-200um.
[0054] The mass ratio of the aluminum-silicon alloy phase change material powder to the high melting point elastic material powder is 1:0.3.
[0055] The stainless steel material is 316 stainless steel (06Cr17Ni12Mo2).
[0056] The aluminum layer is plated on the stainless steel metal by hot-dip plating process, the temperature of the hot-dip aluminum plating liquid is 750° C., and the hot-dip plating time is 10 to 15 minutes.
[0057] The hot-dip aluminum-plated stainless steel metal is placed in the electrolyte of the micro-arc oxidation device, the aluminum-plated stainless steel is used as the anode, and the stainless steel conductor is used as the cathode; the process parameters during the oxidation process are: the current density is controlled at 20A / dm 2 , the oxidation time is 30 minutes and the electrolyte temperature is not higher than 60℃.
[0058] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-temperature phase-change thermal storage ball, characterized in that The steps of the preparation method are: Step 1: Pre-treat the raw materials to ensure that all raw materials are dry and purified to prevent contamination or reaction during the mixing process; use a high-energy ball mill to prepare and mix. Place the aluminum-silicon alloy phase change material powder and the high-melting-point elastic material powder in a container at 30-50°C, and use a high-speed rotating ball or rod to accelerate the mixing process for 5-10 minutes. Mechanical mixing can ensure that the materials are fully and evenly mixed together to obtain the required "core" material. Step 2: Prepare a stainless steel thermal storage spherical shell. First, use hot-dip plating technology to plate aluminum on the stainless steel surface. Then, based on micro-arc processing technology, a dense and uniform aluminum oxide layer is generated on the stainless steel metal surface through an electrochemical process to improve the corrosion resistance of the shell to molten aluminum-silicon alloy. The prepared stainless steel thermal storage spherical shell can maintain stability and long-term durability in a complex working environment, providing reliable protection and support for the storage and application of molten aluminum-silicon alloy. Step 3: Fill the evenly mixed "core" material obtained in step 1 into the stainless steel heat storage sphere shell obtained in step 2 to obtain a high-temperature phase change heat storage sphere with a "shell-core" structure.
2. The method for preparing a high-temperature phase-change thermal storage ball according to claim 1, characterized in that: The aluminum-silicon alloy phase change material is an aluminum-silicon alloy powder with a silicon content of 7-20 wt% and a powder particle size of 50-150 um.
3. The method for preparing a high-temperature phase-change thermal storage ball according to claim 1, characterized in that: The high melting point elastic material is an aluminum oxide (Al2O3) reinforced composite material or a silicon nitride (Si3N4) reinforced composite material, etc., which provides a certain elastic deformation and reduces the stress generated by the volume change of the aluminum silicon alloy during the phase change process; the powder particle size is 20 to 200um.
4. The method for preparing a high-temperature phase-change thermal storage ball according to claim 1, characterized in that: The mass ratio of the aluminum-silicon alloy phase change material powder to the high melting point elastic material powder is 1:0.1-0.
3.
5. The method for preparing a high-temperature phase-change thermal storage ball according to claim 1, characterized in that: The stainless steel material is 300 series stainless steel such as 304 stainless steel (06Cr19Ni10), 310 stainless steel (20Cr25Ni20) and 316 stainless steel (06Cr17Ni12Mo2).
6. The method for preparing a high-temperature phase-change thermal storage ball according to claim 1, characterized in that: The aluminum layer is plated on the stainless steel metal by hot-dip plating process, the temperature of the hot-dip aluminum plating liquid is 750° C., and the hot-dip plating time is 10 to 20 minutes.
7. The method for preparing a high-temperature phase-change thermal storage ball according to claim 1, characterized in that: The hot-dip aluminum-plated stainless steel metal is placed in the electrolyte of the micro-arc oxidation device, the aluminum-plated stainless steel is used as the anode, and the stainless steel conductor is used as the cathode; the process parameters during the oxidation process are: the current density is controlled at 10-20A / dm 2 , the oxidation time is 30 to 70 minutes, and the electrolyte temperature is not higher than 60°C.