Delayed-fracture-resistant 1500MPa-grade cold-rolled martensitic steel and preparation method thereof
Through multi-stage annealing process and chemical composition optimization, the problem of insufficient resistance to delayed fracture performance of cold-rolled martensite steel is solved, and the preparation of martensite steel with high strength and good elongation is achieved, which is suitable for lightweight body applications.
Patent Information
- Application Number
- CN202411240538.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The existing cold-rolled martensitic steel with strength of 1500MPa or above is subject to hydrogen embrittlement limitations in lightweight body applications, resulting in unpredictable failure of tensile strength and difficult to be used in large quantities.
The continuous annealing process is adopted, including multi-stage heating and insulation treatment, combined with slow cooling and fast cooling processes, to control chemical composition and annealing temperature, ensure that the steel structure is completely converted to martensite and improve the resistance to delayed fracture.
The 1500MPa grade cold-rolled martensite steel has been achieved to improve the resistance of delayed fracture performance, meeting the mechanical properties of tensile strength >1500MPa, yield strength 1200MPa~1500MPa, elongation A80≥3% and porosity reaming rate ≥50%, microstructure It is slat-like martensite and performed well in the hydrogen embrittlement sensitivity test.
Smart Images

Figure CN119061243A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steel preparation, and in particular to a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel and a preparation method thereof. Background Art
[0002] With the rapid development of the global automotive industry, lightweighting is of great significance to the energy conservation and emission reduction of automobiles. In addition, for safety reasons, the automotive industry uses a large number of high-strength steel plates. Cold-rolled high-strength steel mainly includes DP steel, DH steel, TRIP steel, CP steel and MS steel, which are mainly achieved by adding alloy elements, increasing the rapid cooling rate, and using phase transformation strengthening. Cold-rolled martensitic steel is a cold-rolled advanced high-strength steel grade, ranging from the lowest 900MPa to the highest strength of 1700MPa. It has ultra-high strength and excellent bending properties, and is usually used in automotive anti-collision beams, bumpers and other parts.
[0003] However, for grades with strengths of 1500MPa and above, it is generally necessary to use a high-strength special annealing production line with water quenching function for production. However, this type of equipment requires a large investment and requires high process stability control. Improper control often leads to serious problems such as poor plate shape and large performance fluctuations. At the same time, ultra-high-strength steel with a strength of 1500MPa and above is particularly sensitive to hydrogen embrittlement, which greatly limits its application in lightweight car bodies. The interaction between hydrogen and different lattice defects significantly reduces the plasticity of hydrogen embrittlement-sensitive materials and leads to unpredictable failures far below the ultimate tensile strength, which makes it difficult to apply the product in large quantities. Summary of the invention
[0004] The present application provides a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel and a preparation method thereof, in order to solve the following technical problem: how to improve the delayed fracture resistance of 1500MPa grade cold-rolled martensitic steel.
[0005] In a first aspect, the present application provides a method for preparing a 1500MPa grade cold-rolled martensitic steel resistant to delayed fracture, the method comprising:
[0006] A cold hardened plate with a set chemical composition is obtained;
[0007] Continuously annealing the chilled plate to obtain a continuously annealed plate;
[0008] The step of continuously annealing the chilled plate to obtain a continuously annealed plate comprises: first heating the chilled plate to a first temperature, and first keeping the temperature under the condition of the first temperature to obtain a first annealed plate;
[0009] The first annealing sheet is heated to a second temperature for a second time, and is kept warm for a second time under the condition of the second temperature, and then slowly cooled and rapidly cooled to obtain a second annealing sheet with a structure completely consisting of martensite;
[0010] Heat the second annealed sheet to a third temperature for over-aging to obtain a continuously annealed sheet;
[0011] Under the condition of a fourth temperature, subject the continuously annealed sheet to a second annealing to obtain a 1500 MPa grade cold-rolled martensitic steel with resistance to delayed fracture.
[0012] Optionally, the first temperature is 640 °C to 680 °C, and the time for the first heat preservation is 30 s to 180 s.
[0013] Optionally, the second temperature is (Ac3 + 10) °C to (Ac3 + 20) °C, and the time for the second heat preservation is 180 s to 360 s.
[0014] Optionally, the heating rate of the first heating is 2 °C / s to 5 °C / s; and / or,
[0015] The heating rate of the second heating is 3 °C / s to 8 °C / s.
[0016] Optionally, the third temperature is 280 °C to 320 °C.
[0017] Optionally, the fourth temperature is 200 °C to 240 °C.
[0018] Optionally, the process parameters of the slow cooling include: the cooling rate is 1 °C / s to 15 °C / s, and the end temperature is Ac1 to Ac3; and / or,
[0019] The process parameters of the rapid cooling include: the cooling medium is a gas containing 50% by volume of hydrogen, and the cooling rate is
[0020] ≥45 °C / s, and the end temperature is 200 °C to 240 °C.
[0021] Optionally, the set chemical composition includes:
[0022] C, Si, Mn, P, S, Cr, Nb, Ti, Cu, Ni, B, N, and Fe; wherein, by mass fraction,
[0023] The content of C is 0.2% to 0.3%, the content of Si is 0.2% to 1.0%, the content of Mn is 2.0% to 3.0%, the content of P is ≤0.015%, the content of S is ≤0.008%, the content of Cr is 0.3% to 0.6%, the content of Nb is 0.01% to 0.04%, the content of Ti is 0.01% to 0.04%, 0 < the content of Cu is ≤0.03%, the content of Ni is 0.01% to 0.05%, the content of B is 0.001% to 0.002%, and the content of N is 0.003% to 0.005%.
[0024] Optionally, obtaining a cold hardened plate with a set chemical composition comprises:
[0025] Continuously casting the molten steel to obtain a slab;
[0026] Heating and rolling the slab with the set chemical composition, and then coiling it to obtain a hot-rolled coil;
[0027] The hot rolled coil is cold rolled to obtain a chilled plate with a set chemical composition; wherein:
[0028] The continuous casting speed is 4m / min to 7m / min, and the thickness of the slab is 110mm to 125mm; and / or,
[0029] The heating temperature is 1120° C. to 1220° C.; and / or,
[0030] The final rolling temperature of the rolling is 890°C to 920°C; and / or,
[0031] The coiling temperature is 550°C to 600°C.
[0032] In a second aspect, the present application provides a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel prepared by the method according to the first aspect,
[0033] The cold-rolled martensitic steel meets the following mechanical properties: tensile strength>1500MPa, yield strength
[0034] 1200MPa~1500MPa, elongation A80≥3%, hole expansion rate≥50%;
[0035] The microstructure of the cold-rolled martensitic steel is entirely lath martensite.
[0036] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0037] The preparation method of the delayed fracture resistant 1500MPa grade cold-rolled martensitic steel provided in an embodiment of the present application comprises: obtaining a chilled plate with a set chemical composition; continuously annealing the chilled plate to obtain a continuously annealed plate; wherein the continuous annealing comprises: first heating the chilled plate to a first temperature, and performing a first heat preservation under the condition of the first temperature to obtain a first annealed plate; second heating the first annealed plate to a second temperature, and performing a second heat preservation under the condition of the second temperature, and then performing slow cooling and rapid cooling to obtain a second annealed plate whose structure is completely martensite; third heating the second annealed plate to a third temperature for overaging; and performing a second annealing on the continuously annealed plate under the condition of a fourth temperature to obtain a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel. The chilled plate with set chemical composition is first heated to a first temperature and then kept warm for a first time, so that the chilled plate can be fully tempered, so that the structure of the chilled plate is uniform, so that the ferrite grains at different parts of the chilled plate will undergo more sufficient recrystallization, and the grain difference of the ferrite will become smaller. At the same time, the martensite will undergo more sufficient tempering and transform into equiaxed ferrite and granular cementite, and the pearlite will also undergo more obvious spheroidization. Since the grain boundary is a fast diffusion channel for carbon atoms, the carbon atoms will gradually diffuse into the original carbon-poor ferrite area during the first heat preservation process, so as to achieve uniform distribution of carbide particles; the second heating to the second temperature and the second heat preservation are carried out, and the structure of the chilled plate is all austenite. The fibrous microstructure completes the recovery and recrystallization process and is completely transformed into austenite. At the same time, the residual cementite is fully dissolved, the various components and microstructures in the austenite are fully homogenized, and the carbides are fully precipitated, thereby improving the delayed fracture resistance; slow cooling can inhibit the formation of new ferrite; rapid cooling can promote the transformation of austenite to martensite, and obtain a structure that is entirely martensitic; the third heating to the third temperature for overaging can temper the martensite, thereby improving the formability and delayed fracture resistance of the cold hardened plate after rapid cooling; the second annealing of the continuously annealed plate under the condition of the fourth temperature can make the hydrogen in the continuously annealed plate escape and improve the delayed fracture resistance. In summary, the delayed fracture resistance of 1500MPa grade cold-rolled martensitic steel is improved through the synergistic effect of chemical composition design, control of continuous annealing process parameters, and the temperature of the second annealing. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0039] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0040] Figure 1 A schematic flow chart of a method for preparing a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel according to some embodiments of the present application;
[0041] Figure 2 A microstructure diagram of a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel provided according to some embodiments of the present application;
[0042] Figure 3 Schematic diagram of U-bending test results of hydrogen embrittlement sensitivity of 1500MPa grade cold-rolled martensitic steel resistant to delayed fracture provided in accordance with some embodiments of the present application. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0044] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0045] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0046] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0047] Figure 1 This is a schematic diagram of a method for preparing a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel according to some embodiments of the present application; see Figure 1 The present application provides a method for preparing a 1500MPa grade cold-rolled martensitic steel with delayed fracture resistance, the method comprising:
[0048] S1, obtaining a cold hardened plate with a set chemical composition;
[0049] In some embodiments, the setting of the chemical composition comprises:
[0050] C, Si, Mn, P, S, Cr, Nb, Ti, Cu, Ni, B, N and Fe; among them, in terms of mass fraction,
[0051] The content of C is 0.2% - 0.3%, the content of Si is 0.2% - 1.0%, the content of Mn is 2.0% - 3.0%, the content of P is ≤0.015%, the content of S is ≤0.008%, the content of Cr is 0.3% - 0.6%, the content of Nb is 0.01% - 0.04%, the content of Ti is 0.01% - 0.04%, 0 < the content of Cu is ≤0.03%, the content of Ni is 0.01% - 0.05%, the content of B is 0.001% - 0.002%, and the content of N is 0.003% - 0.005%.
[0052] In the embodiments of the present application, element C is the most important solid solution strengthening element and the element to improve the hardenability of austenite in martensitic steel. In order to obtain a sufficient amount of martensite during the cooling process to ensure a tensile strength of more than 1500 MPa, at the same time, C forms carbonitrides with microalloying elements Nb and Ti during the heat treatment process, refines the grains, helps to obtain a yield strength of more than 1200 MPa, and avoids the deterioration of welding performance due to too high C content. Exemplarily, the content of the above C can be 0.2%, 0.22%, 0.24%, 0.26%, 0.28%, 0.3%, etc.
[0053] Element Si is also an important solid solution strengthening element. At the same time, Si can effectively promote the enrichment of element C into austenite, improve the hardenability of austenite, purify the ferrite phase, and improve the elongation; Si can also reduce the hydrogen diffusion kinetics and prevent the formation of H2, and inhibit the formation of carbides during the tempering process, thereby improving the delayed fracture performance of the steel plate. However, Si is an important element that causes scale on the surface of hot-rolled plates. Too high Si content will lead to the residue of scale after pickling, which will deteriorate the surface quality of continuous annealing plates. Exemplarily, the content of the above Si can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, etc.
[0054] Mn is an austenite stabilizing element. During the annealing process, it can diffuse from ferrite to austenite, improve the stability of austenite and the hardenability; in addition, Mn can improve the strength of martensite through solid solution strengthening to ensure a high yield strength of more than 1200 MPa and a high tensile strength of more than 1500 MPa. However, Mn increases the sensitivity to delayed fracture. The formation of MnS inclusions often becomes the starting point for the generation of hydrogen-induced cracks. Therefore, the Mn content should not be too high. And too high Mn content is likely to cause tissue segregation, easily lead to forming cracking, deteriorate the comprehensive properties of the steel, and will also enrich on the surface during the annealing process. Therefore, the Mn content should not be too high. Exemplarily, the content of the above Mn can be 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, etc.
[0055] The Cr element can improve the hardenability of austenite in steel, thereby obtaining a sufficient amount of martensite and obtaining a tensile strength of more than 1500MPa, while ensuring that the alloy manufacturing cost is sufficiently low; but at the same time, the Cr element is a ferrite zone expansion element, and too much Cr element will cause the two-phase zone to shrink and hinder the bainite transformation. Exemplarily, the Cr content can be 0.3%, 0.4%, 0.5%, 0.6%, etc.
[0056] The Nb element not only has a significant grain refinement effect, but is also a strong carbide-forming element, which can improve the yield strength of martensitic steel through precipitation strengthening. However, Nb significantly inhibits recrystallization. Too high a Nb content will cause the annealing stage to enter the non-recrystallization zone, resulting in the formation of a deformation band along the rolling direction, resulting in uneven performance. Exemplarily, the above-mentioned Nb content can be 0.01%, 0.02%, 0.03%, 0.04%, etc.
[0057] Like Nb, Ti is also a strong carbide-forming element, which can improve the yield strength through precipitation strengthening. At the same time, Ti is beneficial for refining grains and obtaining a uniform equiaxed microstructure. In addition, the cost of Ti is lower than that of Nb. In addition, the addition of less than 0.01% titanium will cause the steel of the present invention to have low delayed fracture resistance, and the steel of the embodiment of the present application will crack in less than 50 hours during the acid leaching U-bend test. The precipitation of Ti (C, N) promotes the capture of free H, which is conducive to obtaining good delayed fracture resistance. The addition of certain Ti / Nb microalloy elements, the control of the addition of Ni elements, and the residual of certain N elements promote the formation of second phase particles such as Ti (C, N) and NbC, and realize the acquisition of irreversible hydrogen traps; at the same time, after the continuous annealing line is produced, offline low-temperature annealing is carried out to further promote the escape of hydrogen atoms, and finally obtain good delayed fracture resistance. However, excessive addition of Ti leads to increased costs. Exemplarily, the above-mentioned Ti content can be 0.01%, 0.02%, 0.03%, 0.04%, etc.
[0058] As an interstitial solid solution atom, P can appropriately improve the strength of the steel plate, but it is also easy to segregate at the grain boundary and deteriorate the plasticity and formability. For example, the content of P can be 0.015%, 0.013%, 0.010%, etc.
[0059] S is easy to combine with Mn to form coarse MnS inclusions, which deteriorates the delayed fracture resistance of the steel plate. For example, the S content can be 0.008%, 0.007%, 0.006%, etc.
[0060] Cu can improve the strength of steel and its corrosion resistance, but when its content is too high, it will produce hot brittleness. For example, the content of Cu can be 0.03%, 0.02%, 0.01%, etc.
[0061] Ni has a negative impact on delayed fracture resistance, and an ideal steel contains Ni as an impurity level below 0.03%. Exemplarily, the Ni content may be 0.03%, 0.02%, 0.01%, 0.05%, 0.04%, etc.
[0062] B plays a very important role in improving the hardenability of the steel plate during the cooling process. When the B content is too low, it is difficult to achieve grain boundary strengthening, and grain boundary strengthening is required to obtain excellent delayed fracture resistance. In addition, since B diffuses to the grain boundary significantly faster than P, it prevents the adverse effects of P segregation on the grain boundary, which will deteriorate the delayed fracture resistance. However, when the B content is too high, carboride is easily formed, which is not conducive to improving the delayed fracture resistance. Exemplarily, the above-mentioned B content can be 0.001%, 0.0013%, 0.0015%, 0.0018%, 0.002%, etc.
[0063] N can reduce the nitride precipitates in the steel, thereby reducing the formation of irreversible hydrogen trap second phase particles. In addition, it also makes the original austenite grain boundaries coarser, reduces the number of grain boundaries, increases the tendency of crack propagation, and ultimately leads to deterioration of delayed fracture resistance. However, when the N content is too high, the nitrides in the steel coarsen, thereby reducing the grain pinning effect and causing deterioration of the delayed fracture resistance of the steel. Exemplarily, the above-mentioned N content can be 0.003%, 0.0035%, 0.004%, 0.0045%, 0.005%, etc.
[0064] In some embodiments, obtaining a cold hardened plate having a set chemical composition comprises:
[0065] Continuously casting the molten steel to obtain a slab;
[0066] Heating and rolling the slab with the set chemical composition, and then coiling it to obtain a hot-rolled coil;
[0067] The hot rolled coil is cold rolled to obtain a chilled plate with a set chemical composition; wherein:
[0068] The continuous casting speed is 4m / min to 7m / min, and the thickness of the slab is 110mm to 125mm; and / or,
[0069] The heating temperature is 1120° C. to 1220° C.; and / or,
[0070] The final rolling temperature of the rolling is 890°C to 920°C; and / or,
[0071] The coiling temperature is 550°C to 600°C.
[0072] In an embodiment of the present application, the above-mentioned rolling specifically includes: rough descaling, rough rolling, induction heating, fine descaling, finishing rolling, and laminar cooling; the hot-rolled coil can be air-cooled and then cold-rolled; the above-mentioned finishing rolling adopts any one of single-bill rolling, semi-headless rolling and headless rolling, and is based on a multi-mode thin slab continuous casting and rolling production line to prepare delayed fracture resistant 1500MPa grade cold-rolled martensitic steel.
[0073] The casting speed and thickness of the continuous casting are limited to ensure the production rhythm and avoid leakage during endless rolling. For example, the casting speed of the continuous casting can be 4m / min, 5m / min, 6m / min, 7m / min, etc.; the thickness of the slab can be 110mm, 115mm, 120mm, 125mm, etc.
[0074] By limiting the heating temperature, the alloy elements of the slab can be homogenized. By limiting the final rolling temperature of rolling and the temperature of coiling, the structure of the heated slab can be homogenized. Exemplarily, the heating temperature can be 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, etc.; the final rolling temperature of the rolling can be 890°C, 900°C, 910°C, 920°C, etc., and the coiling temperature can be 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, etc.
[0075] S2, continuously annealing the chilled plate to obtain a continuously annealed plate;
[0076] The step of continuously annealing the chilled plate to obtain a continuously annealed plate comprises: first heating the chilled plate to a first temperature, and first keeping the temperature under the condition of the first temperature to obtain a first annealed plate;
[0077] The first annealing sheet is heated to a second temperature for a second time, and is kept warm for a second time under the condition of the second temperature, and then slowly cooled and rapidly cooled to obtain a second annealing sheet with a structure completely consisting of martensite;
[0078] heating the second annealed sheet to a third temperature for overaging to obtain a continuously annealed sheet;
[0079] In some embodiments, the first temperature is 640° C. to 680° C., and the first insulation time is 30 s to 180 s.
[0080] In some embodiments, the second temperature is (Ac3+10)°C to (Ac3+20)°C, and the second insulation time is 180s to 360s.
[0081] In some embodiments, the heating rate of the first heating is 2°C / s to 5°C / s; and / or,
[0082] The heating rate of the second heating is 3°C / s to 8°C / s.
[0083] In the embodiment of the present application, based on the above-mentioned set chemical composition, the process parameters in the continuous annealing are controlled to achieve the optimization of the target structure. The heating rate of the first heating is limited to balance the residence time of the cold hard plate in the continuous annealing furnace, so that the C / Mn elements can be fully diffused, the recovery recrystallization is sufficient, and the structure is homogenized. Exemplarily, the heating rate of the first heating can be 2℃ / s, 3℃ / s, 4℃ / s, 5℃ / s, etc.
[0084] The first heat preservation is carried out under the condition of the first temperature (below Ac1), and the cold-rolled sheet is further subjected to sufficient high-temperature tempering to achieve the purpose of structural homogenization, so that the ferrite grains in different parts will undergo more sufficient recrystallization, and the grain difference of ferrite will become smaller; at the same time, the martensite will undergo more sufficient tempering and transform into equiaxed ferrite and granular cementite; pearlite will also undergo more obvious spheroidization. Since the grain boundary is a fast diffusion channel for carbon atoms, carbon atoms will gradually diffuse to the original carbon-poor ferrite area in the first heat preservation to achieve uniform distribution of carbide particles. Exemplarily, the above-mentioned first temperature can be 640℃, 650℃, 660℃, 670℃, 680℃, etc., and the above-mentioned first heat preservation time can be 30s, 50s, 70s, 100s, 120s, 150s, 170s, 180s, etc.
[0085] The heating rate of the second heating is limited. When heating at a higher temperature, the heating rate needs to be further increased to heat the steel plate to the second temperature in a short time. After heating to above the Ac1 point, the reverse transformed austenite will be evenly distributed in the matrix, thereby eliminating the hereditary unevenness of the original organization. Exemplarily, the heating rate of the second heating can be 6°C / s, 3°C / s, 4°C / s, 5°C / s, 7°C / s, 8°C / s, etc.
[0086] The second insulation (heating stage) is carried out under the condition of the second temperature, so that the structure can be completely austenitized, the fibrous microstructure completes the recovery and recrystallization process, and is completely transformed into austenite, while the residual cementite is fully dissolved, the components and microstructures in the austenite are fully homogenized, and the carbides of Nb and Ti are fully precipitated, so that the required delayed fracture resistance is effectively obtained while ensuring a tensile strength of more than 1500MPa. Exemplarily, the above-mentioned first temperature can be (Ac3+10)℃, (Ac3+12)℃, (Ac3+14)℃, (Ac3+16)℃, (Ac3+180℃, (Ac3+20)℃, etc., and the above-mentioned first insulation time can be 180s, 200s, 220s, 240s, 260s, 280s, 300s, 320s, 340s, 360s, etc.
[0087] In some embodiments, the slow cooling process parameters include: a cooling rate of 1°C / s to 15°C / s, an end point temperature of Ac1 to Ac3; and / or,
[0088] The process parameters of the rapid cooling include: the cooling medium is a gas containing 50% volume fraction of hydrogen, the cooling rate is
[0089] ≥45℃ / s, the end temperature is 200℃~240℃.
[0090] In the embodiment of the present application, the process parameters of slow cooling are limited to ensure that the formation of new ferrite can be suppressed during the initial cooling process, so that not only the evolution of microstructure inhomogeneity can be avoided, but also the reduction of austenite hardenability caused by carbon enrichment in austenite can be avoided. The process parameters of rapid cooling are limited, and the terminal temperature of rapid cooling is below the martensitic phase transformation temperature. Combined with the cooling medium and cooling rate of rapid cooling, austenite is promoted to transform into martensite, and an organizational structure of all martensitic organizations is obtained. Exemplarily, in the above-mentioned slow cooling process parameters, the cooling rate can be 1℃ / s, 3℃ / s, 5℃ / s, 7℃ / s, 9℃ / s, 11℃ / s, 13℃ / s, 15℃ / s, etc.; the terminal temperature can be (Ac3-60)℃, (Ac3-30)℃, (Ac3-40)℃, (Ac3-25)℃, (Ac3-48)℃, etc. Among the above-mentioned rapid cooling process parameters, the cooling rate can be 45°C / s, 46°C / s, 47°C / s, 48°C / s, 49°C / s, etc.; the terminal temperature can be 200°C, 210°C, 230°C, 240°C, etc.
[0091] In some embodiments, the third temperature is 280°C to 320°C.
[0092] In the embodiment of the present application, the overaging treatment is carried out under the condition of the third temperature, which is beneficial to the tempering of martensite, enhancing the plasticity of martensite, and improving the formability and delayed fracture resistance of the finished product. Exemplarily, the third temperature can be 280, 290°C, 300°C, 310°C, 320°C, etc.
[0093] S3. Under the condition of the fourth temperature, the continuously annealed sheet is subjected to a second annealing to obtain a 1500 MPa grade cold-rolled martensitic steel with delayed fracture resistance.
[0094] In some embodiments, the fourth temperature is 200°C to 240°C.
[0095] In the embodiment of the present application, the second annealing is an offline low temperature annealing, which is conducive to the escape of hydrogen and improves the delayed fracture resistance. Exemplarily, the fourth temperature is 200°C, 210°C, 220°C, 230°C, 240°C, etc.
[0096] The present application provides a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel prepared by the method according to the first aspect,
[0097] The cold-rolled martensitic steel meets the following mechanical properties: tensile strength>1500MPa, yield strength
[0098] 1200MPa~1500MPa, elongation A80≥3%, hole expansion rate≥50%;
[0099] The microstructure of the cold-rolled martensitic steel is entirely lath martensite; Figure 2 A microstructure diagram of a delayed fracture resistant 1500MPa grade cold-rolled martensitic steel provided according to some embodiments of the present application; see Figure 2 .
[0100] In the embodiments of the present application, the above-mentioned delayed fracture resistant 1500MPa grade cold-rolled martensitic steel has excellent mechanical properties, and no cracking occurs after being immersed in a 0.1mol / L HCl solution for 300h, and has good U-bend stress corrosion resistance.
[0101] The delayed fracture resistant 1500MPa grade cold-rolled martensitic steel is realized based on the above-mentioned preparation method of the delayed fracture resistant 1500MPa grade cold-rolled martensitic steel. The specific steps of the preparation method of the delayed fracture resistant 1500MPa grade cold-rolled martensitic steel can refer to the above-mentioned embodiment. Since the delayed fracture resistant 1500MPa grade cold-rolled martensitic steel adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.
[0102] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0103] The embodiment of the present application provides a 1500MPa grade cold-rolled martensitic steel with delayed fracture resistance. Please refer to the chemical composition of the 1500MPa grade cold-rolled martensitic steel with delayed fracture resistance shown in Table 1, the preparation process parameters of the cold-hardened plate shown in Table 2, the process parameters of continuous annealing and second annealing of the cold-hardened plate shown in Table 3, and the performance results of the 1500MPa grade cold-rolled martensitic steel with delayed fracture resistance shown in Table 4.
[0104] Table 1 Chemical composition of 1500MPa grade cold-rolled martensitic steel with delayed fracture resistance (wt%)
[0105]
[0106] Table 2 Preparation process parameters of cold hardened plate
[0107]
[0108]
[0109] Table 3 Process parameters of continuous annealing and second annealing of cold hardened plate
[0110]
[0111]
[0112] The delayed fracture resistant 1500 MPa grade cold-rolled martensitic steels prepared in Examples 1 to 6 and Comparative Examples 1 to 4 were subjected to performance tests, see Table 4.
[0113] The tensile strength Rm, yield strength Rp0.2 and A80 in Table 4 are evaluated using GBT 228.1-2021 Metallic Materials Tensile Test Part 1: Room Temperature Test Method. The delayed fracture test evaluation refers to SEP1970-2011, using parallel U-bend state specimens, loading a certain stress, and selecting three parallel specimens for 180-degree bending, clamping bolts, and cleaning the surface with acetone. The test acid solution is replaced with 0.1 mol / L HCl solution every half a month to observe the initiation and development of cracks.
[0114] The hole expansion rate in the above table is based on the ISO16630 standard for the test steel to conduct a hole expansion test (HET). The hole expansion test is used to measure the ability of the material to resist edge rupture during flanging, punching and other processes during the stamping process. The sample size is 100mm×100mm×1.5mm, the initial hole diameter is 10mm, and there are 5 groups of samples for each steel type. At the same time, in order to ensure that the sample is fully fixed by the edge during hole expansion, the distance between the hole center of the expanded sample and the edge of the sample should be no less than 45mm. In order to examine the hole expansion rate of the material under the worst conditions, it is required that the burr direction during hole expansion should be consistent with the direction of punch movement. This hole expansion method can cause the tear zone to deform first, causing microcracks to expand and crack, thereby obtaining the worst edge resistance of the material. The hole expansion rate HER (%) is calculated using the following formula, where df is the hole diameter at the end of hole expansion, and d0 is the initial hole diameter. HER = (df-d0) / d0×100%
[0115] Table 4 Performance results of 1500MPa grade cold rolled martensitic steel resistant to delayed fracture.
[0116]
[0117]
[0118] In summary, the delayed fracture resistant 1500MPa grade cold-rolled martensitic steel prepared by the embodiment of the present application meets the following mechanical properties: tensile strength>1500MPa, yield strength 1200MPa~1500MPa, elongation A80≥3%, hole expansion rate ≥50%; the microstructure of the cold-rolled martensitic steel is all lath martensite. And no cracking occurs after immersion in 0.1mol / L HCl solution for 300h, and it has good resistance to U-bend stress corrosion, exemplary, Figure 3 For a schematic diagram of the U-bend test results of hydrogen embrittlement sensitivity of a 1500MPa grade cold-rolled martensitic steel resistant to delayed fracture provided in accordance with some embodiments of the present application, please refer to Figure 3 However, the C content in Comparative Example 1 is too low, Comparative Example 2 is directly heated to the second temperature, the second temperature of Comparative Example 3 is too low, and Comparative Example 4 does not adopt the second annealing, which makes the performance of the above cold-rolled martensitic steel inferior to that of the embodiment to a certain extent.
[0119] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A preparation method of a 1500 MPa grade cold-rolled martensitic steel with anti-delayed fracture, characterized in that, the method includes: obtaining a cold hard plate with a set chemical composition; continuously annealing the cold hard plate to obtain a continuously annealed plate; the continuously annealing the cold hard plate to obtain a continuously annealed plate includes: first heating the cold hard plate to a first temperature and performing first heat preservation at the first temperature to obtain a first annealed plate; secondly heating the first annealed plate to a second temperature and performing second heat preservation at the second temperature, and then performing slow cooling and rapid cooling to obtain a second annealed plate with a completely martensitic structure; thirdly heating the second annealed plate to a third temperature for overaging to obtain a continuously annealed plate; performing second annealing on the continuously annealed plate at a fourth temperature to obtain a 1500 MPa grade cold-rolled martensitic steel with anti-delayed fracture.
2. The method according to claim 1, characterized in that, the first temperature is 640 °C to 680 °C, and the time of the first heat preservation is 30 s to 180 s.
3. The method according to claim 1, characterized in that, the second temperature is (Ac3 + 10) °C to (Ac3 + 20) °C, and the time of the second heat preservation is 180 s to 360 s.
4. The method according to claim 1, characterized in that, the heating rate of the first heating is 2 °C / s to 5 °C / s; and / or, the heating rate of the second heating is 3 °C / s to 8 °C / s.
5. The method according to claim 1, characterized in that, the third temperature is 280 °C to 320 °C.
6. The method according to claim 1, characterized in that, the fourth temperature is 200 °C to 240 °C.
7. The method according to claim 1, characterized in that, the process parameters of the slow cooling include: the cooling rate is 1 °C / s to 15 °C / s, and the end temperature is Ac1 to Ac3; and / or, the process parameters of the rapid cooling include: the cooling medium is a gas containing 50% by volume of hydrogen, the cooling rate is ≥ 45 °C / s, and the end temperature is 200 °C to 240 °C.
8. The method according to any one of claims 1 to 7, characterized in that, the set chemical composition includes: C, Si, Mn, P, S, Cr, Nb, Ti, Cu, Ni, B, N and Fe; wherein, by mass fraction, the content of C is 0.2% to 0.3%, the content of Si is 0.2% to 1.0%, the content of Mn is 2.0% to 3.0%, the content of P is ≤ 0.015%, the content of S is ≤ 0.008%, the content of Cr is 0.3% to 0.6%, the content of Nb is 0.01% to 0.04%, the content of Ti is 0.01% to 0.04%, 0 < the content of Cu is ≤ 0.03%, the content of Ni is 0.01% to 0.05%, the content of B is 0.001% to 0.002%, and the content of N is 0.003% to 0.005%.
9. The method according to claim 1, characterized in that, The method of obtaining a cold hardened plate with a set chemical composition comprises: Continuously casting the molten steel to obtain a slab; Heating and rolling the slab with the set chemical composition, and then coiling it to obtain a hot-rolled coil; The hot rolled coil is cold rolled to obtain a chilled plate with a set chemical composition; wherein: The continuous casting speed is 4m / min to 7m / min, and the thickness of the slab is 110mm to 125mm; and / or, The heating temperature is 1120° C. to 1220° C.; and / or, The final rolling temperature of the rolling is 890°C to 920°C; and / or, The coiling temperature is 550°C to 600°C.
10. A delayed fracture resistant 1500MPa grade cold-rolled martensitic steel prepared by the method according to any one of claims 1 to 8, It is characterized in that The cold-rolled martensitic steel meets the following mechanical properties: tensile strength>1500MPa, yield strength 1200MPa-1500MPa, elongation A80≥3%, hole expansion ratio ≥50%; The microstructure of the cold-rolled martensitic steel is entirely lath martensite.
Citation Information
Patent Citations
1200MPa cold rolled martensite steel plate and preparation method thereof
CN110592471A
Ultrahigh-strength cold-rolled DH1180 steel and preparation method thereof
CN112095046A
1300MPa-grade ultrahigh-strength cold-rolled steel plate for automobile and manufacturing method thereof
CN113122783A
High-strength steel coil dehydrogenation method
CN114196810A
1100MPa-grade cold-rolled martensitic steel and manufacturing method thereof
CN115044831A
Cited By
1500MPa-grade cold-rolled martensitic steel with high formability and high surface quality for automobile and preparation method thereof
CN121183239A
High-formability and high-surface-quality 1700MPa-grade cold-rolled martensitic steel for automobiles and preparation method thereof
CN121592951A