XBC battery slurry based on Cu and Cu alloy and preparation method thereof
By using Cu and Cu alloy slurry in xBC batteries, combined with Ag-packed Cu powder and Cu alloy powder, the problems of electrode conductivity and manufacturing cost are solved, and efficient conductivity and cost-reducing effect are achieved.
Patent Information
- Application Number
- CN202410863424.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The P-region electrode of xBC battery has problems such as poor ohmic contact effect, large contact resistance and body resistance, and difficult to take into account both manufacturing cost and electrode performance, especially because the Al2O3+SiNx passivation film is difficult to corrode and the aggregation of Al affects the conductivity .
Using xBC battery slurry based on Cu and Cu alloys, the composite Cu powder and Ag powder are used as the conductive phase main body, and the amount of Cu alloy powder is introduced to reduce the Ag usage, and the ratio of Ag wrapped Cu powder and Cu alloy powder is adjusted to reduce the The melting point of Cu avoids the formation of oxide film and improves the sintering effect.
It significantly reduces the manufacturing cost of electrode slurry, improves the conductivity, ensures good contact resistance and line resistance performance, avoids the influence of Cu oxide film, and improves the overall performance of the electrode.
Smart Images

Figure BDA0004919596150000061 
Figure BDA0004919596150000071
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photovoltaic cells and conductive pastes, and in particular to an xBC cell paste based on Cu and Cu alloys and a preparation method thereof. Background Art
[0002] BC is the abbreviation of Back Contact, which means back-contact photovoltaic cells; there are many types of BC cells, such as PBC, IBC, HBC, etc., collectively referred to as xBC cells. Compared with existing TOPCon cells, HJT cells, etc., the biggest feature of xBC is that there is no grid line on the front, and the back is no longer a simple N area or P area, but usually a staggered P and N areas are prepared on the back of the battery, so that the positive and negative electrodes are integrated on the back of the battery. Thanks to this structure, there will be no electrode grid lines blocking the front of the xBC battery, which not only improves the power generation efficiency but also improves the aesthetics of the front. Because BC batteries adopt a design without metal grid lines on the front, the power generation per watt is usually about 2% to 3% higher than that of TOPCon batteries.
[0003] At present, the problem faced by the P-region electrode of xBC battery is that the ohmic contact effect is not good, the contact resistance and body resistance are both large, and it is difficult to balance the manufacturing cost and electrode performance; in addition, since N-type silicon wafers have a higher body life, they can ensure that the non-equilibrium carriers can smoothly reach the back pn junction area before recombination. Therefore, most BC batteries currently use N-type silicon wafers as substrates, and the Al2O3+SiN x The passivation film is difficult to corrode and the "window opening" effect is poor. In addition, in order to control the cost of slurry preparation, more Al and Ag are often co-doped. Although Al has good conductivity, the Al in the electrode is prone to produce Al2O3 oxide film and the finer Al powder is easy to agglomerate and difficult to disperse in the slurry system, which further affects the effect of ohmic contact. Summary of the invention
[0004] In order to solve the above problems, the present invention provides an xBC battery slurry based on Cu and Cu alloy and a preparation method thereof, which better balances the manufacturing cost and comprehensive performance of the xBC battery. The technical solution of the present invention is as follows:
[0005] In a first aspect, the present invention provides an xBC battery slurry based on Cu and Cu alloys, comprising:
[0006] 85-90wt% of a conductive phase; based on the total mass of the conductive phase, it includes 5-65wt% of composite Cu powder, 0-15wt% of Cu alloy powder, and 35-95wt% of Ag powder;
[0007] 3-6 wt% glass phase;
[0008] 0.5-3wt% auxiliary materials;
[0009] The remainder is carrier.
[0010] In one possible implementation,
[0011] The composite Cu powder is a mixture of micron-sized spherical silver-plated Cu powder and micron-sized flaky silver-plated Cu powder. Based on the total mass of the composite Cu powder, the mass proportion of the micron-sized spherical silver-plated Cu powder is 65-70wt%.
[0012] In the above possible implementation, further,
[0013] The D50 particle sizes of the micron-sized flaky silver-coated Cu powder and the micron-sized spherical silver-coated Cu powder are both 0.5 to 1.5 μm.
[0014] In one possible implementation,
[0015] The Cu alloy powder is a mixture of alloy powders formed by Cu and any one and / or two of Ti, Ag and Al.
[0016] In the above possible implementation, further,
[0017] The Cu alloy powder is a mixture of micron-sized spherical Cu alloy powder, micron-sized flaky Cu alloy powder and nano-sized spherical Cu alloy powder;
[0018] The D50 particle size of the micron-sized spherical Cu alloy powder and the micron-sized flaky Cu alloy powder is 1.0 to 2.5 μm, and the D50 particle size of the nano-sized spherical Cu alloy powder is 500 to 800 nm.
[0019] Based on the total mass of the Cu alloy powder, the mass proportion of the nano-scale spherical Cu alloy powder does not exceed 5-10wt%.
[0020] Further,
[0021] Based on the total mass of the Cu alloy powder, the mass of the micron-sized flaky Cu alloy powder does not exceed 20-30wt%.
[0022] In a possible implementation, the glass phase includes a first glass powder and a second glass powder, and based on the total mass of the glass phase:
[0023] The first glass powder comprises 35-60 wt % of Bi2O3, 25-40 wt % of B2O3, and 5-20 wt % of SiO2;
[0024] The mass percentage of the second glass powder is 8-12wt%; the second glass powder is a mixture of at least two of BaO, ZnO, GaO, K2O, and Na2O.
[0025] In a possible implementation, the auxiliary material is a mixture of WO3, metal fluoride and boron powder; based on the total mass of the auxiliary material:
[0026] The content of WO3 is 30-50wt%;
[0027] The metal fluoride content is 10-15wt%;
[0028] The content of the boron powder is 30-45wt%; the D50 particle size of the boron powder is 1-2.5 μm.
[0029] In one possible implementation,
[0030] The carrier includes a mixed solvent and a resin;
[0031] The mixed solvent is a mixture of terpineol and butyl carbitol and / or citric acid, and the mass proportion of the terpineol is ≥60%;
[0032] Based on the total weight of the carrier, the resin comprises 5-8wt% of ethyl cellulose, 0-5wt% of Span series and / or Tween series, 1.5-2.5wt% of sodium dodecylbenzene sulfonate, and 0.2-0.8wt% of polyamide.
[0033] In a second aspect, the present invention provides a method for preparing the above slurry, comprising the following steps:
[0034] S1. Place terpineol in a heating container, maintain the temperature at 45° C., slowly add butyl carbitol and / or citric acid and keep stirring, stir at a stirring speed of 15 rpm for 3 to 5 minutes, so that butyl carbitol and / or citric acid are fully mixed in terpineol to obtain a mixed solvent;
[0035] S2, mixing the various components of the resin evenly, keeping the mixed solvent at 45°C, adding the mixed resin to the mixed solvent, keeping the temperature at 50°C after the resin is completely added, and stirring continuously for 2.5 to 3 hours to make the resin and the mixed solvent fully mixed to form a liquid carrier with a uniform and stable texture, and cooling to room temperature for standby use;
[0036] S3, adding the glass phase and Ag powder into the carrier, stirring and dispersing at a speed of 20 to 30 rpm;
[0037] S4, stirring at a speed of 20 to 30 rpm, mixing the auxiliary materials with the Cu powder and the Cu alloy powder evenly, and then adding them to the carrier, stirring continuously for 8 to 12 hours to obtain a paste;
[0038] S5. Disperse the paste obtained in S4 7 to 8 times, each time for 10 to 20 minutes, to obtain the slurry.
[0039] The above technical solution provided by this application has at least the following technical effects or advantages:
[0040] The xBC battery P-zone slurry disclosed in the present invention uses composite Cu powder and Ag powder as the main body of the conductive phase and introduces an appropriate amount of Cu alloy powder, which greatly reduces the amount of Ag used, thereby significantly controlling the manufacturing cost of the electrode slurry. In addition, the present application also increases the proportion of Ag-coated Cu powder and Cu alloy powder, which, on the one hand, reduces the melting point of Cu in the slurry system, making it easier to carry out the metallization process, and on the other hand, well avoids the situation in which Cu produces an oxide film during sintering and use, thereby affecting the conductive performance. DETAILED DESCRIPTION
[0041] The specific implementation modes of the present invention are described below by way of examples.
[0042] Example 1
[0043] This embodiment provides an xBC battery slurry, including:
[0044] 85wt% of a conductive phase; based on the total mass of the conductive phase, it includes 5wt% of composite Cu powder and 95wt% of Ag powder;
[0045] 3wt% glass phase;
[0046] 1wt% of auxiliary materials;
[0047] The remainder is carrier.
[0048] The composite Cu powder is a mixture of micron-sized spherical Ag-coated Cu powder and micron-sized flaky Ag-coated Cu powder; based on the total mass of the conductive phase, the mass of the micron-sized spherical Ag-coated Cu powder accounts for 70wt%, and the mass of the micron-sized flaky Ag-coated Cu powder accounts for 30wt%; the D50 particle sizes of the micron-sized flaky Ag-coated Cu powder and the micron-sized spherical Ag-coated Cu powder are both 0.5-1.5μm.
[0049] Based on the total mass of the Ag powder, the Ag powder includes 65wt% of micron-sized spherical Ag powder, 30wt% of micron-sized flaky Ag powder and 5% of nanometer-sized spherical Ag powder.
[0050] The glass phase includes a first glass powder and a second glass powder, and according to the total mass of the glass phase:
[0051] The first glass powder comprises 35wt% Bi2O3, 35wt% B2O3, and 20wt% SiO2;
[0052] The mass percentage of the second glass powder is 10wt%; the second glass powder is a mixture of BaO, ZnO, GaO, K2O, and Na2O.
[0053] The auxiliary materials include: 40wt% WO 3, 15wt% of metal fluoride and 45wt% of boron powder; the metal fluoride may be CaF2, AlF3, NaF, etc., and the D50 particle size of the boron powder is 1-2.5μm.
[0054] The carrier includes a mixed solvent and a resin;
[0055] The mixed solvent is a mixture of terpineol, butyl carbitol and citric acid, and the mass proportion of terpineol is 70wt% based on the total mass of the mixed solvent;
[0056] Based on the total mass of the carrier, the resin includes 5wt% of ethyl cellulose, 5wt% of Span series and / or Tween series, 1.5wt% of sodium dodecylbenzene sulfonate, and 0.5wt% of polyamide.
[0057] Example 2
[0058] This embodiment provides an xBC battery slurry, the components of which are substantially the same as those of Embodiment 1, except that:
[0059] The conductive phase includes 65 wt % of composite Cu powder and 35 wt % of Ag powder.
[0060] Example 3
[0061] This embodiment provides an xBC battery slurry, the components of which are substantially the same as those of Embodiment 1, except that:
[0062] The conductive phase includes 45 wt % of composite Cu powder, 45 wt % of Ag powder, and 10 wt % of Cu alloy powder.
[0063] The Cu alloy powder is specifically a mixture of Cu-Ag alloy powder and Cu-Al alloy powder; based on the total mass of the Cu alloy powder, the Cu alloy powder includes 70wt% of micron-sized spherical Cu alloy powder, 20wt% of micron-sized flaky Cu alloy powder and 10wt% of nano-sized spherical Cu alloy powder.
[0064] The D50 particle size of the nano-scale spherical Cu alloy powder is 500-800nm.
[0065] Example 4
[0066] This embodiment provides an xBC battery slurry, the components of which are substantially the same as those of embodiment 3, except that:
[0067] The conductive phase includes 25 wt % of composite Cu powder, 15 wt % of Cu alloy powder, and 60 wt % of Ag powder.
[0068] The preparation methods of the slurries of Examples 1 to 4 are basically the same, and all include the following steps:
[0069] S1. Place terpineol in a heating container, maintain the temperature at 45°C, slowly add butyl carbitol and citric acid and keep stirring, stir at a stirring speed of 15 rpm for 5 minutes to fully mix butyl carbitol and citric acid in terpineol to obtain a mixed solvent;
[0070] S2, mixing the various components of the resin evenly, keeping the mixed solvent at 45°C, adding the mixed resin to the mixed solvent, keeping the temperature at 50°C after the resin is completely added, and stirring for 3 hours to make the resin and the mixed solvent fully mixed to form a liquid carrier with a uniform and stable texture, and cooling to room temperature for standby use;
[0071] S3, adding the glass phase and Ag powder into the carrier, stirring and dispersing at a speed of 20 to 30 rpm;
[0072] S4, stirring at a speed of 20 to 30 rpm, mixing the auxiliary materials with the Cu powder and the Cu alloy powder evenly, and then adding them to the carrier, stirring continuously for 10 hours to obtain a paste;
[0073] S5. Disperse the paste obtained in S4 8 times, each time for 10 to 20 minutes, to obtain the slurry.
[0074] Next, the slurries provided in Examples 1 to 4 are tested to illustrate the beneficial effects of the embodiments of the present application.
[0075] This experiment provides control groups 1 to 6. The slurry components and preparation methods of control groups 1 to 6 are basically the same as those of Example 1, except that:
[0076] Control group 1, whose conductive phase composition is 95wt% Ag powder and 5wt% Al powder;
[0077] Control group 2, whose conductive phase composition is 65wt% Al powder and 35wt% Ag powder;
[0078] Control group 3, whose conductive phase composition is 25wt% Al powder and 75wt% Ag powder;
[0079] Control group 4, whose conductive phase composition is 95wt% Ag powder and 5wt% Cu powder;
[0080] Control group 5, whose conductive phase composition is 65wt% Cu powder and 35wt% Ag powder;
[0081] Control group 6, the conductive phase composition is 25wt% Cu powder and 75wt% Ag powder.
[0082] Using screen printing technology, the slurries of Examples 1 to 4 and the slurries of Control Groups 1 to 6 were printed on silicon wafer substrates to form cells, which were dried in an infrared drying furnace, and then sintered at 740 to 800°C in a belt sintering furnace, and cooled after sintering to form silicon crystalline solar cells. After screen printing and sintering, the cross-section of the metal grid lines of Examples 1 to 4 was close to a Gaussian distribution. The line width was controlled at about 25 μm and the line height was about 5 μm.
[0083] For the prepared batteries, Examples 1 to 4 are designated as S1 to 4, and Control Groups 1 to 6 are designated as D1 to 6, and the contact resistance and line resistance are tested using a TLM contact resistance meter. The test results are shown in Table 1 below:
[0084] Table 1 - Electrical performance test of Examples 1 to 4 and Control Groups 1 to 6
[0085]
[0086]
[0087] From Table 1 we can see that:
[0088] After sintering into electrodes, the slurries provided by S1~S4 basically have relatively ideal line resistance and contact resistance performance. Among them, the electrical performance of S3 and S4 is slightly weaker than that of S1. It has been verified that the reason is that the Cu-Ag alloy is introduced, and the electrical performance is slightly reduced compared with S1, which has a majority of silver content. However, by observing the appearance of the finished electrodes of S1~S4 and the microscopic morphology of the cross section, it is found that the sintering of S3~S4 is better than that of S2. The reason is that the melting point of Cu itself is too high, and it is difficult to completely sinter at conventional sintering temperatures. The alloy component introduced in S3 greatly reduces the melting point of the system, so that the slurry can be fully sintered.
[0089] S2 has a high Cu content, and it is difficult to sinter completely and fully. However, since S2 uses Ag-coated Cu powder, the Ag on its surface can be fully sintered with other components, thus avoiding the incompletely sintered Cu from generating voids in the electrode and causing a significant decrease in electrical performance. Ag and Cu are combined, and their line resistance and contact resistance are better, so the electrical performance of S2 is still within the controllable range and is not seriously affected.
[0090] The line resistance of S2 is higher but the contact resistance is good. The reason is that although Cu is not fully sintered, the Ag coated on its surface can still fill the tiny gaps between the conductive powders after sintering, and the Ag coating can prevent Cu from forming an oxide film, thus obtaining a better contact resistance.
[0091] The contact resistance of S3 and S4 is relatively high, but the line resistance performance is still good. It is speculated that the reason is that they contain Al components. The proportion of Cu-Ag alloy in S4 is higher than that of Cu-Al alloy, so a better line resistance is obtained than that of S3. The content of Ag-coated Cu powder in S3 is higher than that of S3, so a better contact resistance is obtained than that of S4.
[0092] Among D1 to D6, the electrical properties of D1 and D4 are relatively excellent overall. This is because Ag accounts for the vast majority of the slurry mass ratio. However, too high an Ag content will greatly increase the electrode cost, which is not conducive to cost reduction and efficiency improvement.
[0093] The electrical performance of D2 and D3 is inferior to that of S1 to S4. This is because, on the one hand, Al is very easy to form Al2O3 passivation film during sintering and even in the use environment, which itself is easy to affect the electrical performance of the electrode. On the other hand, the Al2O3 passivation film of the electrode affects the ohmic contact with the substrate, further affecting the overall electrical performance of the battery. Especially for D2, its Al content is too high, so the negative impact on the electrical performance is more obvious.
[0094] The electrical performance of D5 and D6 is much worse than that of S1-S4, and even compared with D1-D4. It is verified that the problem is that the Cu content in D5 and D6 is too high, and the melting point of Cu itself is too high (1084.6℃), and it is difficult to fully sinter at a sintering temperature of 740-800℃. Observation of the microscopic morphology shows that a large part of the Cu powder in the electrode is basically not tightly connected with other components, which leads to abnormally high line resistance and contact resistance, which cannot meet the normal use requirements of xBC electrodes.
[0095] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0096] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A xBC battery slurry based on Cu and Cu alloys, characterized in that: include: 85-90 wt% conductive phase; Based on the total weight of the conductive phase, it includes 5-65wt% of composite Cu powder, 0-15wt% of Cu alloy powder, and 35-95wt% of Ag powder; 3-6 wt% glass phase; 0.5-3wt% auxiliary materials; The remainder is carrier.
2. The xBC battery slurry based on Cu and Cu alloy according to claim 1, characterized in that: The composite Cu powder is a mixture of micron-sized spherical silver-coated Cu powder and micron-sized flaky silver-coated Cu powder. Based on the total mass of the composite Cu powder, the mass of the micron-sized spherical silver-coated Cu powder accounts for 65-70wt%.
3. The xBC battery slurry based on Cu and Cu alloy according to claim 2, characterized in that: The D50 particle sizes of the micron-sized flaky silver-coated Cu powder and the micron-sized spherical silver-coated Cu powder are both 0.5 to 1.5 μm.
4. The xBC battery slurry based on Cu and Cu alloy according to claim 1, characterized in that: The Cu alloy powder is a powder of an alloy formed by Cu and at least one of Ti, Ag, and Al.
5. The xBC battery slurry based on Cu and Cu alloy according to claim 4, characterized in that: The Cu alloy powder is a mixture of micron-sized spherical Cu alloy powder, micron-sized flaky Cu alloy powder and nano-sized spherical Cu alloy powder; The D50 particle size of the micron-sized spherical Cu alloy powder and the micron-sized flaky Cu alloy powder is 1.0 to 2.5 μm, and the D50 particle size of the nano-sized spherical Cu alloy powder is 500 to 800 nm. Based on the total mass of the Cu alloy powder, the mass proportion of the nano-scale spherical Cu alloy powder does not exceed 5-10wt%.
6. The xBC battery slurry based on Cu and Cu alloy according to claim 5, characterized in that: Based on the total mass of the Cu alloy powder, the mass of the micron-sized flaky Cu alloy powder does not exceed 20-30wt%.
7. The xBC battery slurry based on Cu and Cu alloy according to claim 1, characterized in that: The glass phase includes a first glass powder and a second glass powder, and according to the total mass of the glass phase: The first glass powder comprises 35-60 wt % of Bi2O3, 25-40 wt % of B2O3, and 5-20 wt % of SiO2; The mass percentage of the second glass powder is 8-12wt%; the second glass powder is a mixture of at least two of BaO, ZnO, GaO, K2O, and Na2O.
8. The xBC battery slurry based on Cu and Cu alloy according to claim 1, characterized in that: The auxiliary material is a mixture of WO3, metal fluoride and boron powder; based on the total mass of the auxiliary material: The content of WO3 is 30-50wt%; The metal fluoride content is 10-15wt%; The content of the boron powder is 30-45wt%; the D50 particle size of the boron powder is 1-2.5 μm.
9. The xBC battery slurry based on Cu and Cu alloy according to claim 1, characterized in that: The carrier includes a mixed solvent and a resin; The mixed solvent is a mixture of terpineol and butyl carbitol and / or citric acid, and the mass proportion of the terpineol is ≥60%; Based on the total weight of the carrier, the resin comprises 5-8wt% of ethyl cellulose, 0-5wt% of Span series and / or Tween series, 1.5-2.5wt% of sodium dodecylbenzene sulfonate, and 0.2-0.8wt% of polyamide.
10. The method for preparing the slurry according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Place terpineol in a heating container, maintain the temperature at 45° C., slowly add butyl carbitol and / or citric acid and keep stirring, stir at a stirring speed of 15 rpm for 3 to 5 minutes, so that butyl carbitol and / or citric acid are fully mixed in terpineol to obtain a mixed solvent; S2, mixing the various components of the resin evenly, keeping the mixed solvent at 45°C, adding the mixed resin to the mixed solvent, keeping the temperature at 50°C after the resin is completely added, and stirring continuously for 2.5 to 3 hours to make the resin and the mixed solvent fully mixed to form a liquid carrier with a uniform and stable texture, and cooling to room temperature for standby use; S3, adding the glass phase and Ag powder into the carrier, stirring and dispersing at a speed of 20 to 30 rpm; S4, stirring at a speed of 20 to 30 rpm, mixing the auxiliary materials with the Cu powder and the Cu alloy powder evenly, and then adding them to the carrier, stirring continuously for 8 to 12 hours to obtain a paste; S5. Disperse the paste obtained in S4 7 to 8 times, each time for 10 to 20 minutes, to obtain the slurry.
Citation Information
Patent Citations
Main grid slurry containing silver-copper alloy powder and preparation method thereof
CN114709003A
Low-temperature slurry for heterojunction photovoltaic cell and preparation method of low-temperature slurry
CN115762850A
Method for metalizing TOPCon solar cell by using silver-coated copper paste and solar cell
CN117650184A
P-region conductive paste for xBC battery, preparation method, electrode and battery
CN118197676A
Copper alloy powder for conductive paste
JP2001131655A