Ion exchange membrane, preparation method thereof and total iron flow battery
By coating polyaniline and TB-COOH layers on the SPEEK base film, the problem of poor ion selectivity of existing ion exchange membranes in all iron flow batteries is solved, the stability and efficiency of the battery are improved, and the higher Capacity retention and battery performance.
Patent Information
- Application Number
- CN202411380446.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing ion exchange membrane has poor ion selectivity in all-iron flow batteries under alkaline conditions, resulting in crossing of redox substances, contaminating the electrolyte, affecting the reliability and durability of the battery, and having a high cost, limiting the Industrialization development.
The polyaniline layer is coated on the surface with a SPEEK base film, and a TB-COOH layer is introduced on the outside of the polyaniline layer to form a SPEEK/polyaniline/TB-COOH structure, which improves the ion selectivity and mechanical stability of the film through hydrogen bonding and Donnan effects. and inhibit cross-contamination of positive and negative electrode iron complexes.
The battery capacity cycle retention rate and battery stability of the full iron flow battery are significantly improved, the water absorption and swelling rate of the film are reduced, the mechanical stability of the film is enhanced, and the Coulomb efficiency and energy efficiency of the battery are improved.
Smart Images

Figure CN119069757A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of batteries, and in particular relates to an ion exchange membrane and a preparation method thereof, and an all-iron liquid flow battery. Background Art
[0002] Redox flow batteries (RFBs) are a promising option for long-term energy storage due to their stability, scalability, and potential reversibility. However, the high cost and low power and energy density of systems using vanadium limit their industrial applications. Utilizing cheap, earth-abundant iron metal is an effective way to reduce costs and improve scalability. All-iron RFBs have the advantages of low chemical toxicity, low material cost, and flexible power and capacity design, making them suitable for long-term energy storage.
[0003] Redox active materials, electrodes and ion exchange membranes (IEMs) are the main components of RFB. For all-iron RFB under alkaline conditions, both the positive and negative electrodes use iron complexes as active materials. The positive electrode is [Fe(CN)6] 3- / [Fe(CN)6] 2- The reaction between the negative electrode is [Fe(TEA)OH] - / [Fe(TEA)(OH)] 2- reactions between them. Carbon-based materials such as carbon felt or graphite felt are often used as electrode materials. Among the main components of RFB, I EMs are a very important part and play a vital role in preventing the crossover of active species and allowing the movement of charge-balancing ions. The I EMs in these systems must meet strict ionic conductivity requirements while limiting the crossover of unwanted reactants.
[0004] However, the poor ion selectivity of existing IEMS inevitably leads to the crossover of redox species between the negative and positive electrolytes. The electrolyte contamination caused by the crossover of redox species can lead to permanent loss of battery capacity efficiency and coulombic efficiency, seriously threatening the reliability and durability of the battery.
[0005] In order to better play the role of the diaphragm and maintain the long-term stability of the alkaline all-iron RFB, IEMs must have excellent physical properties and excellent chemical stability. So far, in order to meet these requirements, the most widely used IEMs are perfluorosulfonic acid membranes (such as Nafion). This type of membrane is composed of a polytetrafluoroethylene (PTFE) hydrophobic chain skeleton with excellent chemical stability and a hydrophilic perfluoroethylene polyether side chain containing a sulfonic acid end group, and has excellent proton conductivity. However, the commonly used Nafion membrane has the problems of poor ion selectivity and high cost, which restricts the development of industrialization. The non-fluorinated ion exchange membrane (sulfonated polyetheretherketone SPEEK) that is currently widely studied has poor chemical stability. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and to provide an ion exchange membrane and a preparation method thereof and an all-iron liquid flow battery.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] An ion exchange membrane comprises a SPEEK base membrane, a polyaniline layer arranged on the surface of the SPEEK base membrane and a TB-COOH layer arranged outside the polyaniline layer.
[0009] The thickness of the SPEEK base film is 50-60 μm; the thickness of the ion exchange membrane is 58-65 μm.
[0010] The present invention also includes a method for preparing the ion exchange membrane, comprising the following steps: 1) preparing a SPEEK base membrane; 2) coating a polyaniline layer on the surface of the SPEEK base membrane to obtain SPEEK / polyaniline; 3) preparing a TB-COOH layer on the surface of the polyaniline layer to obtain SPEEK / polyaniline / TB-COOH.
[0011] The specific steps of step 1) are: adding sulfonated polyetheretherketone SPEEK solid to solvent N,N-dimethylacetamide to prepare a SPEEK solution; forming the obtained SPEEK solution into a film by solution casting method, heating and drying to obtain a SPEEK base film;
[0012] Preferably, the mass volume ratio of sulfonated polyetheretherketone SPEEK solid to solvent N,N-dimethylacetamide is 1 / 5 to 1 / 15 g / mL; preferably 1 / 10 g / mL;
[0013] Preferably, the sulfonated polyetheretherketone SPEEK solid adopts the following steps: dissolving polyetheretherketone PEEK powder in 98wt% concentrated sulfuric acid, the mass volume ratio of polyetheretherketone to concentrated sulfuric acid is between 1 / 5 and 1 / 20 g / mL, and stirring the reaction at a constant temperature of 40 to 50°C for 4 to 7 hours; preferably, the mass volume ratio of polyetheretherketone to concentrated sulfuric acid is 1 / 10 g / mL.
[0014] The specific steps of step 2) are: immersing the SPEEK base film in a solution containing HCl, adding aniline, and then dropping an initiator to induce aniline polymerization, and after the polymerization is completed, obtaining a SPEEK base film coated with a polyaniline layer on the surface;
[0015] Preferably, the molar concentration of the HCl solution is 1-2 mol / L; the added volume of the aniline is 2.5%-10% of the volume of the HCl solution; preferably, the initiator is ammonium persulfate; the added mass of the initiator is 0.15% of the mass of the aniline monomer, and the initiator is dissolved in 1-2 mol / L HCl solution and added dropwise.
[0016] The specific steps of step 3) are: adding TB-COOH solid to the Nafion solution to obtain a TB-COOH suspension; coating the TB-COOH suspension on the SPEEK / polyaniline film by a spin coating method to obtain SPEEK / polyaniline / TB-COOH;
[0017] Preferably, the mass percentage of TB-COOH solid in the Nafion solution is 1 to 5%;
[0018] The volume concentration of the Nafion solution is 1-3%, and the solvent is isopropanol; preferably, the volume concentration of the Nafion solution is 1%.
[0019] The TB-COOH solid is prepared by formula (I);
[0020]
[0021] Specifically, the steps include: dissolving 4-amino-3-methylbenzoic acid in dimethoxymethane DMM, adding trifluoroacetic acid TFA dropwise after the reaction is completely dissolved, slowly pouring a large amount of deionized water under vigorous stirring after the reaction is completed, precipitating a white solid, filtering, washing, and drying to obtain a TB-COOH solid;
[0022] Preferably, the molar ratio of 4-amino-3-methylbenzoic acid to dimethoxymethane DMM is 1:
[0023] (1-10); preferably 1:5.
[0024] The present invention also includes an all-iron liquid flow battery, comprising a positive electrode, a negative electrode, a positive electrode electrolyte, a negative electrode electrolyte and the ion exchange membrane.
[0025] The positive electrode electrolyte is a mixed aqueous solution of positive electrode active material and strong alkali; the positive electrode active material is ferrocyanide [Fe(CN)6] 3- or ferrocyanide [Fe(CN)6] 4- One or two of the following: the concentration of the positive electrode active material is 0.1 to 3 mol / L; the concentration of the strong base in the positive electrode electrolyte is 0.1 to 5 mol / L;
[0026] The negative electrode electrolyte is a mixed aqueous solution of the negative electrode active material and a strong base. The negative electrode active material is iron ions (Fe 3+ ) or ferrous ions (Fe 2+ ) and one or two of the complexes formed with the polyhydroxy complex ligand, and the concentration of the strong base in the negative electrode electrolyte is 0.1 to 5 mol / L.
[0027] The positive electrode active material includes one or more of sodium ferrocyanide, magnesium ferrocyanide, potassium ferrocyanide, sodium ferrocyanide, and magnesium ferrocyanide;
[0028] Preferably, the positive electrode active material is potassium ferrocyanide with a concentration of 0.8 mol / L;
[0029] The negative electrode active material is a complex formed by one or more of ferric chloride, ferric bromide, ferric sulfate, ferric nitrate, ferric phosphate, ferrous chloride, ferrous bromide, ferrous sulfate, ferrous nitrate, and ferrous phosphate and a polyhydroxy complex ligand;
[0030] The polyhydroxy complex ligand is one or more of triethanolamine TEA, 3-[NN-bis(2-hydroxyethyl)amino]-2-hydroxypropanesulfonic acid DIPSO, and bis(2-hydroxyethyl)amino-tris(hydroxymethyl)methane BIS-TRIS.
[0031] Preferably, the negative electrode active material is a complex formed by ferric chloride and triethanolamine TEA, the concentration of ferric chloride is 0.8 mol / L, and the concentration of triethanolamine is 1.6 mol / L. Compared with the prior art, the beneficial effects of the present invention are:
[0032] The present invention provides an ion exchange membrane, wherein a polyaniline intermediate layer containing amino cations is coated on the surface of a SPEEK base membrane, and then a carboxyl-functionalized Troger base TB-COOH is introduced on the surface. Polyaniline is used as the intermediate layer to improve the hydrophilicity of the SPEEK base membrane, and hydrogen bonds exist between the amino group and the sulfonic acid group of the polyaniline to form a conductive channel, thereby reducing the water absorption and swelling rate of the membrane. The negatively charged TB-COOH and the negatively charged positive and negative iron complexes interact with each other through the Donnan effect, thereby suppressing the cross-contamination of the positive and negative iron complexes, improving the selectivity of ions, improving the CE of the all-iron RFB, and improving the capacity cycle retention rate. At the same time, the interaction between the polyaniline intermediate layers is utilized to make the polymer filling denser, the structure stronger, and the mechanical stability of the membrane stronger. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a comparison chart of the performance results of the all-iron liquid flow battery of the embodiment of the present invention and the comparative example;
[0034] Figure 2The graph is a result of the cycle performance of the all-iron liquid flow battery of the embodiment of the present invention and the comparative example. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.
[0036] Example 1
[0037] Preparation process of ion exchange membrane:
[0038] 1) preparing a SPEEK base membrane;
[0039] The preparation method of SPEEK solution is as follows: polyetheretherketone PEEK powder is dissolved in 98wt% concentrated sulfuric acid with a mass volume ratio of 1 / 10g / mL, and the reaction is stirred at a constant temperature of 40-50°C for 4-7 hours; the solution after the reaction is completed is washed with deionized water to neutrality, and dried at 25-100°C to obtain dry SPEEK; the obtained SPEEK is dissolved in a high boiling point organic solvent N,N-dimethylacetamide to prepare a SPEEK solution with a mass volume ratio of 1 / 10g / mL;
[0040] The obtained SPEEK solution was added into a grooved glass plate, and a film was formed by a solution casting method. The film was dried by heating to obtain a SPEEK base film (with a thickness of about 52 μm).
[0041] 2) coating a polyaniline layer on the surface of the SPEEK base film to obtain SPEEK / polyaniline;
[0042] Using SPEEK membrane as the base membrane, the SPEEK membrane was immersed in 20 mL of 1 mol / L HCl solution, and then 0.5 mL of aniline was added and stirred in an ice bath for 3 hours to fully disperse it. Subsequently, a 1 mol / L HCl solution containing 0.75 mg of ammonium persulfate (APS) was added dropwise to induce aniline polymerization, and the mixture was stirred in an ice bath for 12 hours. The SPEEK membrane was taken out and rinsed with deionized water to obtain a polyaniline-coated SPEEK membrane, namely SPEEK / polyaniline.
[0043] 3) preparing a TB-COOH layer on the surface of the polyaniline layer to obtain SPEEK / polyaniline / TB-COOH;
[0044] Preparation of TB-COOH: 4-amino-3-methylbenzoic acid and dimethoxymethane (DMM) are polymerized in trifluoroacetic acid (TFA) in one step to obtain TB-COOH. The reaction equation is shown below:
[0045]
[0046] Under nitrogen atmosphere, 4-amino-3-methylbenzoic acid (1.37 g, 10 mmol) was dissolved in DMM (1.84 mL, 50 mmol). After complete dissolution, it was cooled in an ice bath, and an appropriate amount of TFA (30 mL) was added, dripped for 10 min, and stirred at room temperature for 48 hours. A yellow transparent solution was obtained, and a large amount of deionized water was slowly poured under vigorous stirring to precipitate a white solid. The solid was filtered out and washed with water and ethanol several times until the filtrate became neutral. The white product was collected and dried in a vacuum oven at 120 ° C for 12 hours to obtain TB-COOH.
[0047] 1 wt% TB-COOH powder was added to Nafion solution (Nafion volume concentration 1%), and Nafion solution was used as a binder to obtain TB-COOH suspension. The TB-COOH suspension was coated on the SPEEK / polyaniline film by spin coating to obtain SPEEK / polyaniline
[0048] / TB-COOH-1, thickness is 58 μm.
[0049] Example 2
[0050] 2 wt % TB-COOH was coated on the SPEEK / polyaniline-based film by a spin coating method to obtain SPEEK / polyaniline / TB-COOH-2 with a thickness of 60 μm. The other experimental steps were the same as those in Example 1.
[0051] Example 3
[0052] 4 wt % TB-COOH was coated on the SPEEK / polyaniline-based film by a spin coating method to obtain SPEEK / polyaniline / TB-COOH-4 with a thickness of 62 μm. The other experimental steps were the same as those in Example 1.
[0053] Example 4
[0054] 5 wt % TB-COOH was coated on the SPEEK / polyaniline-based film by a spin coating method to obtain SPEEK / polyaniline / TB-COOH-5 with a thickness of 65 μm. The other experimental steps were the same as those in Example 1.
[0055] Comparative Example 1
[0056] 2 wt % TB-COOH was directly coated on the SPEEK base film by a spin coating method to obtain SPEEK / TB-COOH-2 with a thickness of 55 μm. The other experimental steps were the same as those in Example 1.
[0057] Comparative Example 2
[0058] A Nafion membrane (Nafion 212) with a thickness of 51 μm was used. Other experimental steps were the same as those in Example 1.
[0059] Comparative Example 3
[0060] A SPEEK membrane without any modification was used, with a thickness of 52 μm. Other experimental steps were the same as those in Example 1.
[0061] Comparative Example 4
[0062] The SPEEK membrane directly modified with polyaniline was used, and the thickness was 57 μm. The other experimental steps were the same as those in Example 1.
[0063] The obtained ion exchange membranes of the embodiment and the comparative example are used to prepare all-iron liquid flow batteries:
[0064] The preparation process of the positive electrode electrolyte is as follows: first, 0.08 mol K4[Fe(CN)6] is added to 80 mL of deionized water, and ultrasonicated until the solid is completely dissolved to obtain solution 1; 0.4 mol KOH is weighed and added to solution 1 successively, and stirred continuously to form solution 2; solution 2 is placed in a 100 mL volumetric flask to make up to volume, and 100 mL 0.8 mol / L K4[Fe(CN)6] alkaline solution is obtained for standby use;
[0065] The preparation process of the negative electrode electrolyte is as follows: first, add 0.08 mol FeCl3 to 60 mL deionized water, and sonicate until the solid is completely dissolved to form solution 1; weigh 0.16 mol triethanolamine and dilute it to 25 mL with water, stir evenly, and form solution 2; slowly add solution 2 to solution 1 to form solution 3; weigh 0.4 mol KOH, add it to solution 3 successively, and stir continuously to form solution 4; after cooling solution 4, stir overnight, and make up the volume in a 100 mL volumetric flask to obtain 100 mL triethanolamine (1.6 mol / L)-iron ion (0.8 mol / L) complex solution for standby use.
[0066] The ion exchange membrane, positive electrode electrolyte and negative electrode electrolyte are assembled into a single cell and the charge and discharge performance test is carried out. The battery assembly and test process is as follows:
[0067] 1. Single battery assembly:
[0068] Assemble according to the positive terminal plate, positive current collector, positive graphite felt (6mm*3cm*3cm), ion exchange membrane, negative graphite felt (6mm*3cm*3cm), negative current collector and negative terminal plate.
[0069] Test conditions:
[0070] During battery operation, 100 mA cm -2In the charge and discharge test, the charge and discharge cut-off voltages were 1.7V and 0.5V respectively, and the charge and discharge cycle performance test was performed 100 times.
[0071] Table 1 shows the coulombic efficiency (CE), energy efficiency (EE), voltage efficiency (VE) and capacity decay rate after 100 cycles of Examples 1 to 4 and Comparative Examples 1 to 4.
[0072] Table 1 Performance of alkaline all-iron flow battery
[0073]
[0074] Figure 1 It is a comparison chart of the performance results of the all-iron liquid flow battery of the embodiment of the present invention and the comparative example; Figure 2 The results of the cycle performance of the all-iron liquid flow battery of the embodiment of the present invention and the comparative example are shown in FIG. Figure 1-2 As can be seen from the results in Table 1, in Example 2, after 100 charge and discharge cycle tests, the capacity of the battery decayed by 4.8%, and the EE reached about 90%, indicating that after the ion exchange membrane was modified, the composite membrane was able to inhibit the penetration of ferric ion and ferrous ion complexes through the diaphragm, avoiding cross-contamination of the all-iron RFB electrolyte, improving the CE of the battery, and significantly improving the capacity retention rate.
[0075] Compared with Examples 1 to 4, as the content of TB-COOH coating increases, the water absorption of the membrane increases, which will expand the pore size of the membrane, resulting in a trend of membrane expansion that first decreases and then increases, which is consistent with the CE and capacity retention results. For Comparative Example 1, the TB-COOH coating is directly coated on the surface of the SPEEK membrane. Due to the weak bonding between the SPEEK membrane and the TB-COOH coating, the mechanical stability of the membrane is reduced, and the stability is not significantly improved. For Comparative Example 4, the polyaniline coating is directly coated on the surface of the SPEEK membrane. Due to the hydrogen bonding between the sulfonic acid group of the SPEEK membrane and the amine group of the polyaniline coating, the hydrophilicity is enhanced, resulting in an increase in the membrane swelling rate and a decrease in the ion selectivity of the membrane. Combined with Example 2 and Comparative Example 2, compared with the Nafion 212 ion exchange membrane, the composite membrane of the present invention has a significant improvement in battery stability. The unmodified SPEEK membrane has a capacity decay of about 20% after 100 cycles, further illustrating that the non-perfluorosulfonic acid membrane is less stable than the Nafion membrane.
[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An ion exchange membrane, characterized in that: The invention comprises a SPEEK base film, a polyaniline layer arranged on the surface of the SPEEK base film and a TB-COOH layer arranged outside the polyaniline layer.
2. The ion exchange membrane according to claim 1, characterized in that The thickness of the SPEEK base film is 50-60 μm; the thickness of the ion exchange membrane is 58-65 μm.
3. A method for preparing an ion exchange membrane according to claim 1 or 2, characterized in that: The method comprises the following steps: 1) preparing a SPEEK base film; 2) coating a polyaniline layer on the surface of the SPEEK base film to obtain SPEEK / polyaniline; 3) preparing a TB-COOH layer on the surface of the polyaniline layer to obtain SPEEK / polyaniline / TB-COOH.
4. The method for preparing an ion exchange membrane according to claim 3, characterized in that: The specific steps of step 1) are: adding sulfonated polyetheretherketone SPEEK solid to solvent N,N-dimethylacetamide to prepare a SPEEK solution; forming the obtained SPEEK solution into a film by solution casting method, heating and drying to obtain a SPEEK base film; Preferably, the mass volume ratio of sulfonated polyetheretherketone SPEEK solid to solvent N,N-dimethylacetamide is 1 / 5 to 1 / 15 g / mL; preferably 1 / 10 g / mL; Preferably, the sulfonated polyetheretherketone SPEEK solid adopts the following steps: dissolving polyetheretherketone PEEK powder in 98wt% concentrated sulfuric acid, the mass volume ratio of polyetheretherketone to concentrated sulfuric acid is between 1 / 5 and 1 / 20 g / mL, and stirring the reaction at a constant temperature of 40 to 50°C for 4 to 7 hours; preferably, the mass volume ratio of polyetheretherketone to concentrated sulfuric acid is 1 / 10 g / mL.
5. The method for preparing an ion exchange membrane according to claim 3, characterized in that: The specific steps of step 2) are: immersing the SPEEK base film in a solution containing HCl, adding aniline, and then dropping an initiator to induce aniline polymerization, and after the polymerization is completed, obtaining a SPEEK base film coated with a polyaniline layer on the surface; Preferably, the molar concentration of the HCl solution is 1-2 mol / L; the volume of the added aniline is 2.5%-10% of the volume of the HCl solution; Preferably, the initiator is ammonium persulfate; the added mass of the initiator is 0.15% of the mass of the aniline monomer, and the initiator is dissolved in 1-2 mol / L HCl solution and added dropwise.
6. The method for preparing an ion exchange membrane according to claim 3, characterized in that: The specific steps of step 3) are: adding TB-COOH solid to Nafion solution to obtain TB-COOH suspension; coating the TB-COOH suspension on SPEEK / polyaniline membrane by spin coating method to obtain SPEEK / polyaniline / TB-COOH; Preferably, the mass percentage of TB-COOH solid in the Nafion solution is 1 to 5%; The volume concentration of the Nafion solution is 1-3%, and the solvent is isopropanol; Preferably, the volume concentration of the Nafion solution is 1%.
7. The method for preparing an ion exchange membrane according to claim 6, characterized in that: The TB-COOH solid is prepared by formula (I); Specifically, the steps include: dissolving 4-amino-3-methylbenzoic acid in dimethoxymethane DMM, adding trifluoroacetic acid TFA dropwise after the reaction is completely dissolved, slowly pouring a large amount of deionized water under vigorous stirring after the reaction is completed, precipitating a white solid, filtering, washing, and drying to obtain a TB-COOH solid; Preferably, the molar ratio of 4-amino-3-methylbenzoic acid to dimethoxymethane DMM is 1:(1-10); preferably 1:
5.
8. An all-iron liquid flow battery, characterized in that: It comprises a positive electrode, a negative electrode, a positive electrode electrolyte, a negative electrode electrolyte and the ion exchange membrane according to claim 1 or 2.
9. The all-iron liquid flow battery according to claim 8, characterized in that: The positive electrode electrolyte is a mixed aqueous solution of positive electrode active material and strong alkali; the positive electrode active material is ferrocyanide [Fe(CN)6] 3- or ferrocyanide [Fe(CN)6] 4- One or two of the following: the concentration of the positive electrode active material is 0.1 to 3 mol / L; the concentration of the strong base in the positive electrode electrolyte is 0.1 to 5 mol / L; The negative electrode electrolyte is a mixed aqueous solution of the negative electrode active material and a strong base. The negative electrode active material is iron ions (Fe 3+ ) or ferrous ions (Fe 2+ ) and one or two of the complexes formed with the polyhydroxy complex ligand, and the concentration of the strong base in the negative electrode electrolyte is 0.1~5mol / L.
10. The all-iron liquid flow battery according to claim 9, characterized in that: The positive electrode active material includes one or more of sodium ferrocyanide, magnesium ferrocyanide, potassium ferrocyanide, sodium ferrocyanide, and magnesium ferrocyanide; Preferably, the positive electrode active material is potassium ferrocyanide with a concentration of 0.8 mol / L; The negative electrode active material is a complex formed by one or more of ferric chloride, ferric bromide, ferric sulfate, ferric nitrate, ferric phosphate, ferrous chloride, ferrous bromide, ferrous sulfate, ferrous nitrate, and ferrous phosphate and a polyhydroxy complex ligand; The polyhydroxy complex ligand is one or more of triethanolamine TEA, 3-[NN-bis(2-hydroxyethyl)amino]-2-hydroxypropanesulfonic acid DIPSO, and bis(2-hydroxyethyl)amino-tris(hydroxymethyl)methane BIS-TRIS; Preferably, the negative electrode active material is a complex formed by ferric chloride and triethanolamine TEA, the concentration of ferric chloride is 0.8 mol / L, and the concentration of triethanolamine is 1.6 mol / L.
Citation Information
Cited By
Polyaniline nanofiber felt reinforced sulfonated polyetheretherketone composite proton exchange membrane as well as preparation method and application thereof
CN121065949A
Composite ion conduction membrane for improving ion selective conduction performance through interface design and preparation method of composite ion conduction membrane
CN121394469A