SNN / PVDF flexible piezoelectric sensor and preparation thereof
The preparation of SNN/PVDF flexible piezoelectric sensors through solid phase sintering method and casting method solves the stability of lead-based ferroelectric ceramics in high temperature environments, and realizes lead-free, low-cost and high-sensitivity sensor preparation, suitable for Various application scenarios.
Patent Information
- Application Number
- CN202411256391.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-03
AI Technical Summary
Among existing flexible piezoelectric sensors, lead-based ferroelectric ceramics cause lead-containing oxides to evaporate under high temperature environments, reducing the stability and service life of the device. In addition, traditional preparation methods are costly, expensive equipment or complex processes, making it difficult to achieve lead-free. Wide application of piezoelectric ceramics.
SNN piezoelectric ceramics were prepared by solid phase sintering method, and SNN/PVDF piezoelectric composite film was prepared by casting method. Combined with electrode plating and packaging steps, SNN/ with environmentally friendly, good piezoelectric and high flexibility were produced. PVDF flexible piezoelectric sensor.
It realizes lead-free, low-cost and stable performance SNN/PVDF flexible piezoelectric sensor, with fast response and high sensitivity, is suitable for monitoring pressure and acceleration signals, and has broad application prospects.
Smart Images

Figure CN119072211A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of flexible sensors, and in particular to a SNN / PVDF flexible piezoelectric sensor and its preparation. Background Art
[0002] With the rapid development of information technology, people's demand for flexible piezoelectric sensors is gradually increasing. Flexible piezoelectric sensors can be fitted with various complex structures, sensitively converting various external signals in the interaction between human body, objects and environment into electrical signals, and finally realizing flexible perception of multi-dimensional space. At the same time, due to the self-powered and lightweight characteristics of piezoelectric materials, the device also has the advantages of low power consumption, high sensitivity and lightweight. Flexible piezoelectric sensors have always been a hot topic in research and application.
[0003] The key components that flexible piezoelectric sensors rely on are piezoelectric materials that can monitor and respond to changes in the surrounding environment in real time. In the development of modern sensor technology, 0-3 piezoelectric composite materials have become a widely used piezoelectric sensitive element due to their unique properties. This material is composed of high-performance piezoelectric ceramic particles and other polymers. By precisely controlling the composition, proportion and preparation process of the material, it can be ensured that the material is suitable for various applications, such as biomedicine, automotive safety systems, industrial monitoring and other fields, and ensure high sensitivity, high-speed response and high reliability during use, showing great application potential and value.
[0004] The high temperature environment of lead-based ferroelectric ceramics also causes the volatilization of lead oxides, reducing the stability and service life of the device. Therefore, lead-free piezoelectric ceramics are urgently needed to be developed. 2 NeA 5 O 15 , referred to as SNN) is a lead-free piezoelectric ceramic with a tungsten bronze structure. It has a high Curie temperature, good ferroelectric properties, strong spontaneous polarization, large optical nonlinearity, and has great application potential in the field of dielectric energy storage. Polyvinylidene fluoride (PVDF) piezoelectric polymer has the characteristics of good flexibility, stable chemical properties, and excellent ductility, but its piezoelectric coefficient is smaller than that of piezoelectric ceramics. The 0-3 type piezoelectric composite material prepared by compounding SNN with PVDF will have flexibility, high piezoelectricity and high sensitivity.
[0005] There are many methods for preparing SNN / PVDF flexible piezoelectric sensors, including magnetron sputtering, vapor deposition, sol-gel method, spin coating and tape casting. Among them, although magnetron sputtering can improve the uniformity of thin films and can deposit large-area thin films, it is costly and the equipment is expensive; vapor deposition can realize the preparation of multi-component thin films, but the size is not controllable; the sol-gel method is simple in process, but it is easy to damage the material during high-temperature sintering; the spin coating method is limited to mass production and is prone to waste of raw materials. In contrast, the tape casting method is low-cost, simple to operate, and suitable for industrial production. Most importantly, this method can prepare thin films with different component ratios according to performance requirements, and can also prepare laminated composite materials. Therefore, the tape casting method is an ideal choice for preparing SNN / PVDF flexible piezoelectric sensors.
[0006] In summary, the present invention provides a SNN / PVDF flexible piezoelectric sensor and a preparation method thereof. Summary of the invention
[0007] The purpose of the present invention is to provide a SNN / PVDF flexible piezoelectric sensor and a preparation method thereof. The present invention uses a traditional solid-phase sintering method to prepare SNN piezoelectric ceramics, uses a tape casting process to prepare SNN / PVDF piezoelectric film, and then undergoes a series of steps such as electrode plating, polarization, and packaging to produce an environmentally friendly, good piezoelectric, high flexibility, and fast-response SNN / PVDF flexible piezoelectric sensor.
[0008] The present invention is achieved by the following steps:
[0009] 1) SrCO 3 、Na 2 CO 3 , Nb 2 O 5 As raw materials, SNN piezoelectric ceramic powder was synthesized by solid phase sintering method based on stoichiometric ratio;
[0010] 2) Preparation of SNN / PVDF piezoelectric composite film by tape casting;
[0011] 3) Electrode plating on SNN / PVDF film;
[0012] 4) Package the SNN / PVDF piezoelectric sensor.
[0013] Preferably, in step 1), the preparation of the SNN piezoelectric ceramic powder specifically comprises the following steps:
[0014] 11) SrCO 3 、Na 2 CO 3 , Nb 2 O 5The three drugs were placed in a blast drying oven and dried at 50-80℃ for 10-30min.
[0015] 12) Accurately weigh SrCO and 3 、Na 2 CO 3 , Nb 2 O 5 The three drugs were placed in a ball mill, and appropriate amount of anhydrous ethanol was added and ball milled in a planetary ball mill for 12-24 hours;
[0016] 13) The mixed solution obtained by ball milling was dried in an oven at 90°C and then sieved;
[0017] 14) The sieved raw materials are placed in a muffle furnace for pre-sintering. The pre-sintering conditions are: heating to 1150°C for 3 hours and then keeping the temperature for 12 hours. After pre-sintering, the raw materials are sieved again to obtain the piezoelectric ceramic powder required for the subsequent preparation of SNN / PVDF film.
[0018] Preferably, in step 2), the preparation of the SNN / PVDF piezoelectric composite film specifically comprises the following steps:
[0019] 21) Weigh polyvinylidene fluoride (PVDF) powder and dissolve it in N,N-dimethylformamide (DMF) solution in a mass ratio of 1:19 to 1:9. Place the mixed solution in a magnetic stirrer and stir for 3 to 6 hours. Set the temperature to 40 to 60°C and the rotation speed to 200 to 500 r / min to obtain a PVDF transparent solution.
[0020] 22) Mix the SNN powder and the PVDF transparent solution in a mass ratio of 1:19~1:4, and place it in a magnetic stirrer for stirring again. Set the temperature to 40~60℃ and the speed to 200~500r / min to finally obtain a white colloidal SNN / PVDF mixed solution.
[0021] 23) After the SNN / PVDF mixed solution is prepared, it can be poured onto the glass plate of the casting machine for casting. After the solution is evenly cast, the glass plate is placed horizontally in a drying oven at 40~60℃ and dried for 3~6 hours, waiting for the DMF component in the SNN / PVDF solution to evaporate, and finally the desired film is obtained.
[0022] Preferably, in step 3), the electrode plating of the SNN / PVDF film specifically comprises the following steps:
[0023] 31) Cut the film to obtain a rectangular sample of 2 cm × 3 cm;
[0024] 32) Copper foils are attached to the two surfaces of the rectangular film sample as the bottom electrode and top electrode of the flexible piezoelectric sensor, and the area of the copper foil is controlled to be slightly smaller than the surface area of the SNN / PVDF piezoelectric film;
[0025] Preferably, in step 4), the packaging of the SNN / PVDF film specifically includes the following steps: bonding copper wires on both sides of the film sample using conductive glue, and packaging with a PDMS film to reduce damage to the sensor caused by external friction, moisture, etc.
[0026] The flexible piezoelectric sensor provided by the present invention includes: a flexible piezoelectric film layer, which provides a piezoelectric effect for the sensor to ensure the induction and conversion of external signals; a flexible electrode layer, which is located on the upper and lower surfaces of the flexible piezoelectric film layer; and a flexible packaging layer, which is located on the upper and lower surfaces of the flexible piezoelectric film layer with the electrode layer, and is used to resist interference from external signals and prevent loss and damage to the sensor caused by external friction, moisture, etc.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The material selected for the present invention is lead-free SNN piezoelectric ceramics, which are harmless to the environment and human body and have low cost; the SNN piezoelectric ceramics have stable performance, high Curie temperature, good dielectric ferroelectric properties, and have great application potential in the field of dielectric energy storage; the selected preparation process is relatively simple and efficient, and can realize the preparation of SNN / PVDF flexible piezoelectric sensors of any size and shape; the produced SNN / PVDF flexible piezoelectric sensor is environmentally friendly, has good piezoelectricity, high flexibility, and can respond quickly and resist impact, and has broad application prospects in the monitoring of pressure and acceleration signals. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a schematic diagram of the structure of a SNN / PVDF flexible piezoelectric sensor provided by the present invention;
[0030] Figure 2 It is the microscopic morphology and hysteresis loop of SNN / PVDF flexible piezoelectric film;
[0031] Figure 3 It is the output comparison between SNN / PVDF flexible piezoelectric sensor and standard accelerometer;
[0032] Figure 4 is the output response of the SNN / PVDF flexible piezoelectric sensor at different frequencies; DETAILED DESCRIPTION
[0033] The present invention is further described in detail below through specific embodiments and drawings.
[0034] Experimental Example 1
[0035] This experimental example is used to illustrate the preparation method of the SNN / PVDF flexible piezoelectric sensor, and is performed according to the following steps:
[0036] 1) SrCO 3 、Na 2 CO 3 , Nb 2 O 5 The three drugs were placed in a blast drying oven and dried at 60°C for 30 min.
[0037] 2) Accurately weigh SrCO and 3 、Na 2 CO 3 , Nb 2 O 5 The three drugs were placed in a ball mill, and appropriate amount of anhydrous ethanol was added and ball milled in a planetary ball mill for 24 h;
[0038] 3) The mixed solution obtained by ball milling was dried in an oven at 90°C and then sieved;
[0039] 4) The sieved raw materials are placed in a muffle furnace for pre-sintering. The pre-sintering conditions are to increase the temperature to 1150°C for 3 hours and keep it warm for 12 hours. After pre-sintering, the raw materials are sieved again to obtain the piezoelectric ceramic powder required for the subsequent preparation of SNN / PVDF film.
[0040] 5) Weigh polyvinylidene fluoride (PVDF) powder and dissolve it in N,N-dimethylformamide (DMF) solution in a mass ratio of 1:19. Place the mixed solution in a magnetic stirrer and stir for 4 h. Set the temperature to 50°C and the speed to 300 r / min to obtain a PVDF transparent solution.
[0041] 6) SNN powder and PVDF solution were mixed in a mass ratio of 1:19, and stirred in a magnetic stirrer again. The temperature was set to 50°C and the speed was set to 300 r / min. Finally, a white colloidal SNN / PVDF mixed solution was obtained.
[0042] 7) After the SNN / PVDF mixed solution is prepared, it can be poured onto the glass plate of the casting machine for casting. After the solution is evenly cast, the glass plate is placed horizontally in a drying oven at 50°C and dried for 5 hours, waiting for the DMF component in the SNN / PVDF solution to evaporate, and finally the desired film is obtained.
[0043] 8) Cut the film to obtain a rectangular sample of 2 cm × 3 cm;
[0044] 9) Copper foils are attached to the two surfaces of the rectangular film sample as the bottom electrode and top electrode of the flexible piezoelectric sensor, and the area of the copper foil is controlled to be slightly smaller than the surface area of the SNN / PVDF piezoelectric film;
[0045] 10) After polarization, copper wires were glued to both sides of the film sample using conductive glue and then encapsulated with PDMS film to finally obtain the SNN / PVDF flexible piezoelectric sensor. According to the proportion of SNN piezoelectric ceramic powder in the total mass of SNN / PVDF solution, the sensor sample was named 5%SNN / PVDF.
[0046] Experimental Example 2
[0047] This embodiment is carried out in a similar manner to Experimental Example 1, except that in step 6), the mass ratios of the SNN powder and PVDF solution used are 1:9, 3:17, and 1:4, respectively. The sensors finally prepared are named 10% SNN / PVDF, 15% SNN / PVDF, and 20% SNN / PVDF, respectively.
[0048] Experimental Example 3
[0049] Based on the four flexible piezoelectric sensors provided in Experimental Examples 1 and 2 above, this experimental example detects the output response of the sensor. Specifically, the following steps are performed:
[0050] 1) The flexible piezoelectric sensor is fixed on the vibration table. The sinusoidal signal from the function generator is amplified by the power amplifier and introduced into the vibration table to generate the required vibration signal. The vibration table can also provide a certain acceleration to the flexible piezoelectric sensor at the working frequency.
[0051] 2) The output charge signal of the sensor is further amplified by the preamplifier, then collected by a data acquisition card (DAQ card) and transmitted to a laptop computer;
[0052] 3) A commercial accelerometer is required as a calibration reference at room temperature during the test so that the manufactured sensor can be compared with it;
[0053] Figure 3 Output comparison between SNN / PVDF flexible piezoelectric sensor and standard accelerometer;
[0054] 4) Keeping other conditions unchanged, adjust the frequency of the sinusoidal signal on the function generator to 50Hz, 100Hz, 150Hz, and 200Hz, and observe and record the output response of the flexible piezoelectric sensor, such as Figure 4 shown.
[0055] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. A person skilled in the art may modify or make equivalent substitutions for the technical solutions of the present invention without departing from the spirit and scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A method for preparing a SNN / PVDF flexible piezoelectric sensor, characterized in that: The following steps are involved: 11) Using SrCO3, Na2CO3 and Nb2O5 as raw materials, the SNN piezoelectric ceramic powder was synthesized by solid phase sintering method based on the stoichiometric ratio; 12) Prepare SNN / PVDF piezoelectric composite film by tape casting; 13) Electrode plating on SNN / PVDF film; 14) Package the SNN / PVDF piezoelectric sensor.
2. The method for preparing the SNN / PVDF flexible piezoelectric sensor according to claim 1, characterized in that: In step 11), the preparation of the SNN piezoelectric ceramic powder specifically includes the following steps: 21) Place SrCO3, Na2CO3 and Nb2O5 in a forced air drying oven respectively, and then dry them at 50-80℃ for 10-30min; 22) According to the mass ratio of 10:1:20, accurately weigh SrCO3, Na2CO3, and Nb2O5 using an electronic balance and place them in a ball mill. Add appropriate amount of anhydrous ethanol and mill in a planetary ball mill for 12-24 hours. 23) The mixed solution obtained by ball milling was dried in an oven at 90°C and then sieved; 24) The sieved raw materials are placed in a muffle furnace for pre-sintering. The pre-sintering conditions are: heating to 1150°C for 3 hours and then keeping warm for 12 hours. After pre-sintering, the raw materials are sieved again to obtain the piezoelectric ceramic powder required for the subsequent preparation of SNN / PVDF film.
3. The method for preparing the SNN / PVDF flexible piezoelectric sensor according to claim 1, characterized in that: In step 12), the preparation of the SNN / PVDF piezoelectric composite film specifically includes the following steps: 31) Weigh polyvinylidene fluoride (PVDF) powder and dissolve it in N,N-dimethylformamide (DMF) solution in a mass ratio of 1:19 to 1:9, and place the mixed solution in a magnetic stirrer for 3 to 6 hours at a temperature of 40 to 60 °C and a rotation speed of 200 to 500 r / min to obtain a PVDF transparent solution; 32) Mix the SNN powder and the PVDF transparent solution in a mass ratio of 1:19~1:4, and stir them in a magnetic stirrer again. Set the temperature to 40~60℃ and the speed to 200~500r / min, and finally obtain a white colloidal SNN / PVDF mixed solution; 33) After the SNN / PVDF mixed solution is prepared, it can be poured onto the glass plate of the casting machine for casting. After the solution is evenly cast, the glass plate is placed horizontally in a drying oven at 40-60°C and dried for 3-6 hours, waiting for the DMF component in the SNN / PVDF solution to evaporate, and finally the desired film is obtained.
4. The method for preparing the SNN / PVDF flexible piezoelectric sensor according to claim 1, characterized in that: In step 13), the SNN / PVDF film electrode is plated, specifically comprising the following steps: 41) Cut the film into rectangular samples of 2 cm × 3 cm; 42) Copper foils are pasted on both surfaces of the rectangular film sample as the bottom electrode and top electrode of the flexible piezoelectric sensor. The copper foil area is controlled to be slightly smaller than the surface area of the SNN / PVDF piezoelectric film.
5. The method for preparing the SNN / PVDF flexible piezoelectric sensor according to claim 1, characterized in that: In step 14), the SNN / PVDF piezoelectric sensor is packaged, specifically including the following steps: copper wires are glued on both sides of the film sample using conductive glue, and the film is packaged with a PDMS film to reduce damage to the sensor caused by external friction, moisture, etc.