Environment-friendly water-based wood modifier as well as preparation method and application thereof
By using environmentally friendly water-based wood modifiers of vinyl monomers, oxalic acid and silanes, combined with vacuum-impregnation-pressurization treatment and moisture-curing technology, the problem of wood and bamboo easily absorb moisture and regaining moisture in high humidity environments is solved, and the size is significantly improved Stability and biological durability, and efficient prevention and control of molds and termites, ensuring the outdoor use performance of wood and bamboo.
Patent Information
- Application Number
- CN202411294559.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
AI Technical Summary
Existing wood and bamboo modification methods are prone to moisture absorption and moisture recovery in high humidity environments, and are difficult to completely cure, resulting in dimensional instability and insufficient biological durability, especially when used outdoors, which are prone to mildew, decay and termite erosion.
The environmentally friendly water-based wood modifier is used, and the composition includes vinyl monomer, oxalic acid and silane. The wood and bamboo are treated by vacuum-impregnation-pressurization or vacuum-pressurization impregnation method, and combined with heating and moisture curing technology, a macromolecular polymer is formed in wood. Self-polymerization and substitution reactions on bamboo cell walls fill micro-vacuums and block channels, improving dimensional stability and bio-durability.
Significantly improves the dimensional stability and biological durability of wood and bamboo in high humidity environments, prevents mold, decay and termite erosion, retains the original color and texture, and can effectively prevent and control Aspergillus niger, Trichoderma, and Penicillium tangerine Infection with cyanobacteria has achieved 100% prevention and control effect.
Smart Images

Figure CN119077878A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an environmentally friendly water-based wood modifier, a preparation method and application thereof, and belongs to the technical field of wood and bamboo material protection modification. Background Art
[0002] Forests are one of the most important resources on earth, and they are the foundation for the sustained, rapid and healthy development of the national economy. They play an irreplaceable role in economic construction and sustainable development. Forests are also the basis of biodiversity, not only providing a variety of valuable wood and raw materials for production and life, but also providing a variety of food for human life. More importantly, forests can regulate the climate, maintain water and soil, prevent and alleviate natural disasters such as drought, flood, wind and sand, and purify the air and eliminate noise.
[0003] Wood and bamboo (referred to as wood and bamboo) are used in outdoor furniture, floors, plank roads, fences and house exterior wall panels. They are easily attacked by mold, decay fungi and even termites, causing discoloration, decay, insect infestation, cracking and deformation. As a result, wood and bamboo materials give people an uncomfortable experience when used in outdoor places, and their market share is replaced by other materials.
[0004] Wood and bamboo materials have the characteristics of high strength-to-weight ratio, excellent mechanical properties, strong processability, beautiful color, warm touch, etc., and are widely used in furniture and home decoration, indoor and outdoor floors, wooden plank roads, etc. In particular, my country's abundant fast-growing wood and special bamboo resources can be modified to improve their physical, mechanical and biological durability, and use them in outdoor places is an effective means to expand the scope of their resource application.
[0005] At present, there are three main treatment methods for outdoor wood and bamboo materials: 1) anti-corrosion and anti-mildew treatment; 2) heat treatment of wood and bamboo materials; 3) low molecular weight resin modification of wood. Anti-corrosion and anti-mildew treatment is to use anti-corrosion and anti-mildew agents that are toxic in themselves to impregnate wood and bamboo materials, mainly CCA, ACQ and copper azole. This method has relatively low cost, good effect and simple process. However, after these copper-based preservatives are used to treat wood, the wood turns green and the color becomes uneven when used outdoors. In addition, the anti-corrosion wood is prone to cracking and deformation during outdoor application. Heat treatment is also the main method to improve the durability and dimensional stability of wood and bamboo materials. This method is environmentally friendly and does not add any agents to wood and bamboo materials, but its durability improvement effect is not obvious, and it is difficult to meet the needs of long-term outdoor use. Compared with the first two methods, the low-molecular-weight resin modification of wood is relatively complicated. It mainly uses low-molecular-weight chemical reagents to impregnate wood and bamboo materials, and then heats them to complete self-polymerization in the cell cavity and cell wall of the wood and bamboo materials or react with the hydroxyl groups of the cell wall of the wood and bamboo materials, occupying and blocking the water in and out of the wood channels, reducing the water absorption of wood, and improving the dimensional stability and biological durability of wood. The main ones are low-molecular-weight phenolic resins, furfuryl alcohol resins, etc. The biggest challenge faced by this type of method is the curing process. Wood and bamboo materials absorb the modifier through impregnation mainly through axial tissues such as ducts. There is a gradient in the distribution of the agent from the end to the core. During the thermal curing process, the resin at the end often solidifies first, which leads to problems such as the moisture inside the wood and bamboo materials cannot be exported from the wood and bamboo materials, and the resin in the core cannot be completely cured.
[0006] The use of vinyl monomers to modify wood and bamboo completely retains the original color, texture and feel of the wood after modification, and can significantly improve the dimensional stability and outdoor durability of wood and bamboo. However, there is a significant problem of moisture absorption when used in high humidity environments. Therefore, it is urgent to further optimize the stability of polymers based on the vinyl monomer modification method. Summary of the invention
[0007] The present invention provides an environmentally friendly water-based wood modifier, a preparation method thereof and a use thereof. The environmentally friendly water-based wood modifier of the present invention can be used for forest pest control or for forest wood pest control modification; it can effectively solve the problem that vinyl monomer modified wood and bamboo materials are easy to absorb moisture and regain moisture in a high humidity environment, and significantly improve the dimensional stability and outdoor durability of wood and bamboo materials.
[0008] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:
[0009] An environmentally friendly water-based wood modifier, whose raw material components include vinyl monomer, oxalic acid, silane and water, wherein the mass proportion of the vinyl monomer is 4% to 14%, the mass proportion of oxalic acid is 0.7% to 3%, the mass proportion of silane is 2.5% to 8%, and water is the balance.
[0010] The sum of the masses of the above vinyl monomer, oxalic acid, silane and water is 100%.
[0011] In the present invention, "%" refers to mass percentage unless otherwise specified.
[0012] The environmentally friendly water-based wood modifier of the invention uses water as a solvent, is environmentally friendly, safe and has low cost.
[0013] As one of the preferred implementation schemes, in the above-mentioned environmentally friendly water-based wood modifier, the mass proportion of vinyl monomer is 12% to 14%, the mass proportion of oxalic acid is 2.3% to 2.4%, the mass proportion of silane is 7.6% to 7.8%, and water is the balance.
[0014] In order to better ensure the preparation effect, the vinyl monomer is at least one of acrylamide, ethyl methacrylate or N-hydroxymethyl acrylamide. More preferably, the vinyl monomer is a mixture of acrylamide, ethyl methacrylate and N-hydroxymethyl acrylamide in a mass ratio of 1: (0.3-0.6): (0.2-0.5).
[0015] In order to further improve the preparation effect, the silane is 3-aminopropyltriethoxysilane (silane coupling agent KH550).
[0016] The preparation method of the environmentally friendly water-based wood modifier is as follows: vinyl monomer, oxalic acid and silane are added into water and stirred evenly to obtain the environmentally friendly water-based wood modifier.
[0017] The environmentally friendly water-based wood modifier can be used for preventing wood and bamboo materials from mildew, corrosion and termites.
[0018] The wood and bamboo materials in this application include wood, bamboo and related integrated materials.
[0019] The above preparation can be used for preventing wood and bamboo from mildew, corrosion and termites; it can also be used for wood and bamboo modification to solve the problems of existing wood and bamboo panels being prone to mildew, decay and termite infestation in outdoor applications.
[0020] When used for wood and bamboo modification, vacuum-impregnation-pressure impregnation, vacuum-pressure impregnation or normal pressure immersion is used to treat wood and bamboo, and then wet-cured, chemical reactions occur in wood and bamboo cells and cell walls, thereby filling micro-voids in the cell walls of wood and bamboo, blocking channels, and swelling the cell walls of wood and bamboo. It can be used for the modification of outdoor floors, plank roads, wall hangings and other panels.
[0021] In order to ensure the treatment effect, the above-mentioned vacuum-impregnation-pressure impregnation treatment method is as follows: put the wood and bamboo materials into the impregnation tank, treat them for 14 to 16 minutes under the condition of a vacuum degree of -0.07 to -0.09 MPa, then inhale the environmentally friendly water-based wood modifier, and then increase the pressure in the tank to 1.4 to 1.6 MPa, maintain the pressure for 1 hour, release the pressure and soak at normal pressure for 1 hour, take out the wood and bamboo materials and let them stand horizontally to air dry for 60 to 72 hours to obtain the impregnated wood and bamboo materials.
[0022] In order to ensure the treatment effect, the vacuum-pressure impregnation method is as follows: the wood and bamboo materials and the environmentally friendly water-based wood modifier are placed in an impregnation tank, and the treatment is carried out for 20 to 40 minutes under the condition of a vacuum degree of -0.07 to -0.09 MPa, and then the pressure in the tank is increased to 1.4 to 1.6 MPa, and the pressure treatment is maintained for 1 hour, and the pressure is released and the normal pressure is soaked for 1 hour, and the wood and bamboo materials are taken out and horizontally placed to air dry for 60 to 72 hours to obtain the impregnated wood and bamboo materials;
[0023] In order to ensure the treatment effect, the above-mentioned normal pressure impregnation method is: place the wood and bamboo materials and the environmentally friendly water-based wood modifier in an impregnation tank, soak them under normal pressure for 36 to 48 hours, take them out and let the wood and bamboo materials stand horizontally and air-dry for 10 to 12 hours to obtain the impregnated wood and bamboo materials.
[0024] In the above vacuum-impregnation-pressure impregnation method, vacuum-pressure impregnation method or normal pressure immersion method, the amount of environmentally friendly water-based wood modifier used is based on immersing the wood and ensuring sufficient impregnation margin (that is, after the impregnation or soaking is completed, the environmentally friendly water-based wood modifier can still immerse the wood).
[0025] In order to ensure the uniformity of curing and the modification effect, the wet curing is as follows: the impregnated wood and bamboo materials are wrapped and sealed with aluminum foil or high-temperature resistant plastic, and then heated and cured at a temperature of 100-120°C for 2-4 hours, and then the temperature is reduced to 50°C and reacted for 8-12 hours to obtain mildew-proof, anti-corrosion and termite-proof wood and bamboo materials as outdoor wood and bamboo boards.
[0026] The environmentally friendly water-based wood modifier can be used for the prevention and control of Aspergillus niger, and the prevention and control efficacy of Aspergillus niger reaches 100%.
[0027] The environmentally friendly water-based wood modifier can be used for the prevention and control of Trichoderma viride, and the prevention and control efficacy of Trichoderma viride reaches 100%.
[0028] The environmentally friendly water-based wood modifier can be used for the prevention and control of Penicillium citrinum, and the prevention and control efficacy of Penicillium citrinum reaches 100%.
[0029] The environmentally friendly water-based wood modifier can be used for the prevention and control of blue stain fungi, and the prevention and control efficacy of blue stain fungi reaches 100%.
[0030] The above-mentioned environmentally friendly water-based wood modifier can be used for the prevention and control of decay fungi and inhibit them, so that wood and bamboo materials can reach a strong corrosion resistance level.
[0031] The technologies not mentioned in the present invention are all referred to the prior art.
[0032] The environmentally friendly water-based wood modifier of the present invention adopts vinyl monomer as the modifier matrix, and is compounded with organic acid and silane to form a preparation. The organic acid used is analyzed in a small amount and has no irritating odor. It can be used for mildew prevention of wood and bamboo, and / or for corrosion prevention of wood and bamboo, and / or for termite prevention of wood and bamboo. When used for mildew, corrosion and termite prevention modification of forest wood, the vinyl monomer, organic acid and silane undergo self-polymerization reaction on the cells and cell walls of the wood and bamboo through heating, and undergo substitution reaction with the hydroxyl groups on the cell walls to generate macromolecules that swell the cell walls, thereby reducing the water absorption of the wood and bamboo. , filling the micro-voids in the cell wall of wood, blocking the channels, and swelling the cell wall of wood, thereby improving the dimensional stability and biological durability of wood and bamboo materials; at the same time, vinyl monomers, organic acids, and silanes form an interpenetrating network structure inside the wood and bamboo materials, making the polymer more stable, greatly improving the moisture absorption and moisture regain of vinyl monomer-modified wood and bamboo materials in a high humidity environment; and retaining the original color, texture, and texture of the wood, with good uniformity; can be completely cured; can be used for the prevention and inhibition of Aspergillus niger, Trichoderma viride, Penicillium citrinum, blue stain fungi and / or decay fungi; simple components, easy preparation, and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a physical comparison diagram of untreated wood and the modified wood in Example 2 (in the figure, a is untreated wood; b is modified wood).
[0034] Figure 2 The longitudinal sections of the untreated wood and the modified wood in Example 2 are microscopic morphologies (the left picture is the untreated wood; the right picture is the modified wood).
[0035] Figure 3 The figure shows the aging resistance of the untreated wood and the wood modified in Example 2 after 4 months of field near-ground exposure test (the left figure shows the untreated wood; the right figure shows the modified wood).
[0036] Figure 4 The untreated wood and the modified wood of Example 2 are shown in Figure 4 after being infected by mold and blue stain fungi for 4 weeks (in the figure, A is the untreated wood infected by Aspergillus niger for four weeks; B is the modified wood infected by Aspergillus niger for four weeks; C is the untreated wood infected by blue stain fungi for 4 weeks; Figure D is the modified wood infected by blue stain fungi for four weeks).
[0037] Figure 5 The figures show the untreated wood and the modified wood of Example 2 after being infected by decay fungi for 4 weeks (the left picture shows the untreated wood, and the right picture shows the modified wood). DETAILED DESCRIPTION
[0038] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0039] Embodiment 1:
[0040] A method for modifying a wood board is carried out according to the following steps:
[0041] 1. Environmentally friendly water-based wood modifier
[0042] Vinyl monomer, oxalic acid and 3-aminopropyltriethoxysilane (silane coupling agent KH550) are added into water and stirred evenly to obtain an environmentally friendly water-based wood modifier, wherein the mass percentage of the vinyl monomer is 13%; the mass percentage of oxalic acid is 2.4%; the mass percentage of silane is 7.8%, and water is the balance. The vinyl monomer is a mixture of acrylamide, ethyl methacrylate and N-hydroxymethyl acrylamide in a mass ratio of 1:0.5:0.3.
[0043] 2. Vacuum-impregnation-pressure impregnation treatment of wood
[0044] Put red pine wood with a size of 550mm×100mm×20mm into an impregnation tank, treat it for 15 minutes under a vacuum degree of -0.08MPa, then absorb the environmentally friendly water-based wood modifier to immerse the wood, and ensure sufficient impregnation margin, then increase the pressure in the tank to 1.5MPa, maintain the pressure for 1h, release the pressure and soak it at normal pressure for 1h, take out the wood and place it horizontally for 72h under the conditions of temperature of 22-25℃ and humidity of 60%, and obtain the impregnated wood, and the weight gain rate of the wood is greater than 25%.
[0045] 3. Moisture curing
[0046] The impregnated wood after being air-dried is wrapped and sealed with aluminum foil, and then heated and cured at a temperature of 100-110° C. for 3 hours, and then the temperature is reduced to 50° C. and reacted for 12 hours to obtain a modified outdoor wood board.
[0047] Embodiment 2:
[0048] The difference between this embodiment and the first embodiment is that the impregnation method in step 2 is a vacuum-pressure impregnation method, specifically: the wood and the environmentally friendly water-based wood modifier are placed in an impregnation tank, the modifier immerses the wood, and a sufficient impregnation margin is ensured, the treatment is carried out for 30 minutes under the condition of a vacuum degree of -0.08MPa, and then the pressure in the tank is increased to 1.5MPa, the pressure is maintained for 1 hour, the pressure is released and the soaking is carried out at normal pressure for 1 hour, and the wood is taken out and horizontally placed at a temperature of 22-25°C and a humidity of 60% for 72 hours to obtain the impregnated wood, and the weight gain rate of the wood is greater than 25%. The rest is the same as the first embodiment.
[0049] Figure 1 This is a physical comparison between unmodified and modified wood. As can be seen from the picture, there is no obvious difference in appearance between the two. The modified wood retains the original color, texture and feel of the wood.
[0050] Figure 2 The longitudinal sections of unmodified and modified wood are microscopic morphologies. The left picture is unmodified wood, with no attachments on the cell walls, transparent pores, and traces of fiber breakage on the section. The right picture is modified wood, with obvious chemicals attached to the cell walls, and chemicals gathered at the edges of the pores. The section end is smooth, indicating that the chemicals have also penetrated into the cell walls.
[0051] Figure 3 This is the aging resistance of unmodified and modified wood after 4 months of field near-ground exposure test. The left picture is the untreated wood, which shows a color change to dark gray with obvious signs of mildew and decay. The right picture is the modified wood, which still maintains good wood texture and color, with no signs of mildew and decay.
[0052] Figure 4 Figure 4 shows the condition of unmodified and modified wood after being infected by mold and blue stain fungi for 4 weeks. In the figure, A shows the condition of untreated wood after being infected by Aspergillus niger for four weeks. It is severely infected by mold and the anti-mildew efficacy is 0; B shows the condition of modified wood after being infected by Aspergillus niger for four weeks, without any signs of mold infection; C shows the condition of untreated wood after being infected by blue stain fungi for 4 weeks, and the entire sample is severely blue-stained; Figure D shows the condition of modified wood after being infected by blue stain fungi for four weeks, without any signs of blue stain.
[0053] Figure 5 The left picture shows the unmodified and modified wood after being infected by decay fungi for 4 weeks. The untreated wood is severely infected by decay fungi, with a weight loss rate of more than 45%, which is a non-corrosion-resistant grade. The right picture shows the modified wood after being infected by decay fungi for 4 weeks. There are no signs of decay fungi infection, and the weight loss rate is less than 10%, which is a strong corrosion-resistant grade.
[0054] Embodiment three:
[0055] The difference between this embodiment and the first embodiment is that the impregnation method in step 2 is a normal pressure impregnation method, specifically: the wood and the environmentally friendly water-based wood modifier are placed in an impregnation tank, the modifier immerses the wood and ensures the impregnation margin, and the wood is immersed in the normal pressure condition for 48 hours, and the wood is taken out and horizontally placed at a temperature of 22 to 25° C. and a humidity of 60% for air drying for 12 hours to obtain the impregnated wood, and the weight gain rate of the wood is greater than 10%. The rest is the same as the first embodiment.
[0056] Embodiment 4:
[0057] The difference between this embodiment and the second embodiment is that the wood material in step 2 is bamboo material, and the weight gain rate of the bamboo material after impregnation is greater than 10%. The rest is the same as the second embodiment.
[0058] Embodiment five:
[0059] The difference between this embodiment and the second embodiment is that the vinyl monomer is acrylamide. The rest is the same as the second embodiment.
[0060] Embodiment six:
[0061] The difference between this embodiment and the second embodiment is that the vinyl monomer is ethyl methacrylate. The other parts are the same as the second embodiment.
[0062] Embodiment seven:
[0063] The difference between this embodiment and the second embodiment is that the vinyl monomer is N-hydroxymethyl acrylamide. The other parts are the same as the second embodiment.
[0064] Comparative Example 1:
[0065] The difference between this embodiment and the second embodiment is that the mass percentage of the vinyl monomer is 3%, the mass percentage of oxalic acid is 0.5%, the mass percentage of silane is 2.1%, and water is the balance. The rest is the same as the second embodiment.
[0066] Comparative Example 2:
[0067] The difference between this embodiment and the second embodiment is that the mass percentage of the vinyl monomer is 15%, the mass percentage of oxalic acid is 3.5%, the mass percentage of silane is 9%, and water is the balance. The rest is the same as the second embodiment.
[0068] Comparative Example 3:
[0069] The difference between this embodiment and the second embodiment is that the vinyl monomer is styrene and water is the balance. The rest is the same as the second embodiment.
[0070] All of the above examples retain the original color, texture and feel of the wood, are fully cured, and are uniform inside and out.
[0071] According to the national standards GB / T 18261-2013 "Test method for the efficacy of mildew inhibitors on wood mildew and discoloration fungi" and GB / T 18260-2015 "Laboratory test method for the toxicity of wood preservatives to termites", the untreated wood (CK1), untreated bamboo (CK2), and the wood or bamboo obtained in each case were tested for mildew resistance and termite resistance. The flexural strength and flexural modulus of each case were tested with reference to the national standards GB / T1936.1-2009 "Test method for flexural strength of wood" and GB / T 1936.2-2009 "Test method for flexural modulus of elasticity of wood". The test results are as follows:
[0072]
[0073]
[0074] Note: Aspergillus niger V.Tiegh;
[0075] Green Trichoderma: Trichoderma viride Pers.ex Fr;
[0076] Penicillam citrinum Thom;
[0077] Botryodiplodia theobromae Pat
[0078] White rot fungus: Trametes versicolor;
[0079] Brown rot fungus: Gloeophyllum trabeum.
Claims
1. An environmentally friendly water-based wood modifier, characterized in that: Its raw material components: It includes vinyl monomer, oxalic acid, silane and water, wherein the mass proportion of vinyl monomer is 4% to 14%, the mass proportion of oxalic acid is 0.7% to 3%, the mass proportion of silane is 2.5% to 8%, and water is the balance.
2. The environmentally friendly water-based wood modifier according to claim 1, characterized in that: The mass proportion of the vinyl monomer is 12% to 14%, the mass proportion of oxalic acid is 2.3% to 2.4%, the mass proportion of silane is 7.6% to 7.8%, and water is the balance.
3. The environmentally friendly water-based wood modifier according to claim 1 or 2, characterized in that: The vinyl monomer is at least one of acrylamide, ethyl methacrylate or N-hydroxymethyl acrylamide; and the silane is 3-aminopropyltriethoxysilane.
4. The environmentally friendly water-based wood modifier according to claim 3, characterized in that: The vinyl monomer is a mixture of acrylamide, ethyl methacrylate and N-hydroxymethyl acrylamide in a mass ratio of 1: (0.3-0.6): (0.2-0.5).
5. A method for preparing the environmentally friendly water-based wood modifier according to any one of claims 1 to 4, characterized in that: Add vinyl monomer, oxalic acid and silane into water and stir evenly to obtain an environmentally friendly water-based wood modifier.
6. Use of the environmentally friendly water-based wood modifier according to any one of claims 1 to 4, characterized in that: Used for preventing wood and bamboo from mildew and decay, and / or for preventing wood and bamboo from termites.
7. The use according to claim 6, characterized in that: The environmentally friendly water-based wood modifier according to any one of claims 1 to 5 is used to treat wood and bamboo materials by vacuum-impregnation-pressure impregnation method, vacuum-pressure impregnation method or normal pressure immersion method to obtain impregnated wood and bamboo materials, which are then wet-cured to obtain mildew-proof, anti-corrosion and anti-termite wood and bamboo materials.
8. The use according to claim 7, characterized in that: The vacuum-impregnation-pressure impregnation treatment method is as follows: the wood and bamboo materials are placed in an impregnation tank, and the treatment is carried out for 14 to 16 minutes under the condition of a vacuum degree of -0.07 to -0.09 MPa, and then an environmentally friendly water-based wood modifier is inhaled, and then the pressure in the tank is increased to 1.4 to 1.6 MPa, and the pressure treatment is maintained for 1 hour, and the pressure is released and the normal pressure is soaked for 1 hour, and the wood and bamboo materials are taken out and horizontally placed to air dry for 60 to 72 hours to obtain the impregnated wood and bamboo materials; The vacuum-pressure impregnation method is as follows: the wood and bamboo materials and the environmentally friendly water-based wood modifier are placed in an impregnation tank, and the treatment is carried out for 20 to 40 minutes under the condition of a vacuum degree of -0.07 to -0.09 MPa, and then the pressure in the tank is increased to 1.4 to 1.6 MPa, and the pressure treatment is maintained for 1 hour, and the pressure is released and the bamboo materials are immersed in normal pressure for 1 hour, and the wood and bamboo materials are taken out and placed horizontally to air dry for 60 to 72 hours to obtain the impregnated wood and bamboo materials; The normal pressure impregnation method is as follows: the wood and bamboo materials and the environmentally friendly water-based wood modifier are placed in an impregnation tank, immersed for 36 to 48 hours under normal pressure conditions, and the wood and bamboo materials are taken out and placed horizontally to air dry for 10 to 12 hours to obtain the impregnated wood and bamboo materials.
9. The use according to claim 7 or 8, characterized in that: Wet curing is as follows: the impregnated wood and bamboo materials are wrapped and sealed with aluminum foil or high temperature resistant plastic, and then heat-cured at a temperature of 100-120°C for 2-4 hours, and then the temperature is lowered to 50°C and reacted for 8-12 hours to obtain mildew-proof, anti-corrosion and termite-proof wood and bamboo materials.
10. Use of the environmentally friendly water-based wood modifier according to any one of claims 1 to 4, characterized in that: Used for the prevention and inhibition of Aspergillus niger, and / or for the prevention and inhibition of Trichoderma viride, and / or for the prevention or inhibition of Penicillium citrinum, and / or for the prevention and inhibition of blue stain fungi, and / or for the prevention and inhibition of decay fungi.
Citation Information
Cited By
Modified bamboo wood and preparation method and application thereof
CN120962806A
Modified bamboo material, and preparation method and application thereof
CN120962806B