Environment-friendly rubber composite material of polydopamine / KH550 modified carbon nanotube and preparation method of environment-friendly rubber composite material
By modifying single-wall carbon nanotubes with polydopamine/KH550, the problem of difficult to take into account both the dielectric constant and loss of silicone rubber materials is solved, and a silicone rubber composite material with high mechanical properties and excellent dielectric properties is achieved, which expands its application field.
Patent Information
- Application Number
- CN202411201329.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
While the existing silicone rubber materials increase the dielectric constant, the dielectric loss is high, which limits its application range. The aggregation and winding of single-wall carbon nanotubes in the material lead to uneven performance.
Single-walled carbon nanotubes are modified by polydopamine/KH550, formed by non-covalent π-π interaction and hydrogen bonding, and are uniformly dispersed in silicon rubber, improving the mechanical and dielectric properties of the material.
It significantly improves the mechanical strength, thermal stability and dielectric properties of composite materials, reduces dielectric losses, meets a wider application needs, and is simple in preparation, environmentally friendly, low in cost, and is convenient for industrial production.
Smart Images

Figure CN119081412A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of rubber materials, and in particular to an environmentally friendly rubber composite material of polydopamine / KH550 modified carbon nanotubes and a preparation method thereof. Background Art
[0002] Silicone rubber (SR) has many excellent properties due to its special chemical structure. Its main chain is mainly composed of silicon-oxygen bonds (-Si-O-), which have a high bond energy (about 466±33kJ / mol), much higher than the bond energy of carbon-carbon bonds (CC) and carbon-oxygen bonds (CO) (335~356kJ / mol). This enables silicone rubber to maintain structural stability in high and low temperature environments, while having strong chemical corrosion resistance. Because its molecular main chain is in a helical configuration and the molecular chain is more flexible, silicone rubber has high flexibility. This series of characteristics of silicone rubber makes it widely used in automotive interiors, building materials, industrial manufacturing, and medical materials. Although its physical and mechanical properties are inferior to those of some materials, its high and low temperature resistance and wide operating temperature range (up to -100℃~350℃) are its important advantages.
[0003] Single-walled carbon nanotubes (SWCNTs) have completely different structural characteristics. They are composed of carbon atoms connected by strong CC covalent bonds to form a graphene grid structure with almost no defects. The diameter of single-walled carbon nanotubes is usually between 1 and 6 nm, and the length can reach micrometers, with an aspect ratio of up to 100 to 1000. Due to its extremely high axial tensile strength (about 100 times that of steel) and low density (about 1.2 to 2.1 g cm -3 , which is one-seventh of steel or even lower), single-walled carbon nanotubes are very suitable as a reinforcing phase for composite materials. Single-walled carbon nanotubes have extremely high mechanical and mechanical strength. Their theoretical Young's modulus can reach 1000GPa, far exceeding diamond, and their elastic modulus can reach 1TPa, which is similar to diamond. The elastic strain is between 5% and 12%, which is much higher than steel. These characteristics make single-walled carbon nanotubes very suitable for reinforcing polymers, and can significantly improve the strength, hardness and durability of composite materials.
[0004] Silicone rubber performs well in electrical insulation, mechanical properties, aging resistance and high temperature resistance, but the low dielectric constant of pure silicone rubber limits its application. In order to improve the dielectric constant, researchers usually use the method of adding conductive fillers. Carbon nanotubes have attracted much attention due to their unique structure and properties. However, the addition of carbon nanotubes may lead to an increase in the dielectric loss of the material, which is not conducive to practical applications. Therefore, how to reduce the dielectric loss while improving the dielectric constant of the material has become the focus and difficulty of current research. Summary of the invention
[0005] The present application is made in view of the above-mentioned problems. The present application provides an environmentally friendly rubber composite material of polydopamine / KH550 modified carbon nanotubes and a preparation method thereof, which realizes the effective combination of silicone rubber and single-walled carbon nanotubes. The prepared composite silicone rubber has good environmental protection, high mechanical strength and excellent dielectric properties.
[0006] The first aspect of the present application provides a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material, comprising the following raw materials in parts by weight: 100 parts of silicone rubber, 2 to 8 parts of hydroxy silicone oil, 30 to 160 parts of carbon black, 0.5 to 2 parts of vulcanizing agent, 3 to 7 parts of silane coupling agent, 1 to 5 parts of single-walled carbon nanotubes, 1 to 5 parts of dopamine, and 1 to 5 parts of KH550.
[0007] The second aspect of the present application also provides a method for preparing an environmentally friendly rubber composite material of polydopamine / KH550 modified carbon nanotubes, comprising the following steps:
[0008] (1) uniformly dispersing single-walled carbon nanotubes in deionized water, adding a certain amount of dopamine for deposition polymerization, and after the reaction is completed, washing, filtering, and drying to obtain polydopamine-modified single-walled carbon nanotubes;
[0009] (2) After KH550 is hydrolyzed, single-walled carbon nanotubes modified with polydopamine are added, and after the reaction, the single-walled carbon nanotubes are filtered and dried to obtain surface functionalized single-walled carbon nanotubes;
[0010] (3) Weigh corresponding weights of silicone rubber, silane coupling agent and hydroxy silicone oil, and mix them evenly in an internal mixer at high speed; add carbon black and the modified single-walled carbon nanotubes in (2) and mix them to obtain a silicone rubber compound.
[0011] (4) After the silicone rubber mix has cooled, add the vulcanizer on the open mill, pass it through thinly, let the colloid stand for a period of time after it cools down, and finally perform compression molding.
[0012] In any embodiment, the preparation method specifically comprises the following steps:
[0013] (1) dispersing single-walled carbon nanotubes uniformly in deionized water by ultrasonic oscillation, and adding a buffer solution to stabilize the pH of the single-walled carbon nanotube suspension within a certain range; then, adding a certain amount of dopamine to the solution, and after the room temperature deposition polymerization reaction is completed, washing, filtering, and drying to obtain polydopamine-modified single-walled carbon nanotubes;
[0014] (2) After KH550 and deionized water are hydrolyzed in a three-necked flask under certain conditions, single-walled carbon nanotubes modified with polydopamine are added, the reaction is continued, and finally, the single-walled carbon nanotubes with surface functionalization are obtained by filtering and drying;
[0015] (3) Weigh corresponding weights of silicone rubber, silane coupling agent and hydroxy silicone oil, and stir them evenly in an internal mixer at high speed; add carbon black in batches, and stir thoroughly after each addition; add the modified single-walled carbon nanotubes in batches and ensure that they are evenly mixed; when the temperature rises to 140 to 170° C., evacuate the mixture and stir for 1 to 3 hours to obtain a silicone rubber compound;
[0016] (4) After cooling to room temperature, add vulcanizing agent on the open mill and pass it thinly for 3 to 5 times. After the colloid cools to room temperature, let it stand for more than 15 hours; the mixed rubber is molded at 140 to 160°C for 10 to 20 minutes and 10 to 20 MPa.
[0017] In any embodiment, the buffer solution used in step (1) is a tris(hydroxymethyl)aminomethane-hydrochloric acid mixed solution, and the pH range of the buffer solution is 5.5-8.
[0018] In any embodiment, the deposition reaction time of dopamine in step (1) is 10 to 24 hours. The thickness of the dopamine deposition layer can be adjusted according to different deposition times.
[0019] In any embodiment, the ratio of the single-walled carbon nanotubes to dopamine used in step (1) is 1:1-3.
[0020] In any embodiment, in step (2), the mass ratio of KH550 to polydopamine-modified single-walled carbon nanotubes is 1:1-3, the reaction temperature is 40-60° C., and the reaction time is 3-6 hours.
[0021] In any embodiment, the silicone rubber in step (3) is methyl vinyl silica gel with a molecular weight of 450,000 to 700,000, wherein the vinyl content is 0.1% to 3%; the mass ratio of the modified single-walled carbon nanotubes to the silicone rubber is 1 to 10:100.
[0022] In any embodiment, the hydroxy silicone oil in step (3) is α,ω-dihydroxypolydimethylsiloxane, and the dynamic viscosity is 30 to 40 mPa.s.
[0023] In any embodiment, the silane coupling agent in step (3) is at least one of vinyltriethoxysilane, vinyltrimethoxysilane, and vinyltri(β-methoxyethoxy)silane.
[0024] In any embodiment, the vulcanizing agent in step (3) is one of benzoyl peroxide, diisopropylbenzene peroxide, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0025] Beneficial effects of the present invention:
[0026] (1) The present invention significantly improves the performance of the composite material by modifying single-walled carbon nanotubes using polydopamine / KH550. The present invention effectively reduces the aggregation and entanglement of single-walled carbon nanotubes in silicone rubber by grafting single-walled carbon nanotubes with polydopamine and KH550, making them uniformly dispersed in the polymer matrix. The addition of polydopamine-modified single-walled carbon nanotubes significantly improves the mechanical properties and thermal stability of the silicone rubber composite material.
[0027] (2) Polydopamine has a stable structure and can be attached to almost any inorganic or organic interface without destroying the original structure of the material. Polydopamine is adsorbed on the surface of single-walled carbon nanotubes through non-covalent π-π interactions, and has the characteristics of high efficiency, simple composition, and mild reaction conditions, thus achieving surface modification of single-walled carbon nanotubes. KH550 grafted on the surface of polydopamine has many amino groups, which not only increases the spacing between carbon nanotubes, but also forms hydrogen bonds with the substrate molecular chain, thereby effectively improving the overall performance of the composite material and meeting a wider range of application needs.
[0028] (3) The preparation method of the polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material of the present application is simple, green and environmentally friendly, low in cost, and easy to industrialize. The polydopamine modified carbon nanotubes can form an effective reinforced network structure in the rubber matrix, thereby increasing the mechanical strength and wear resistance of the material. In addition, the polydopamine modified carbon nanotubes also have good thermal conductivity, which can improve the thermal stability of the rubber material and reduce the deformation and aging rate under high temperature conditions. By adding polydopamine modified carbon nanotubes, the mechanical properties and thermal stability of the rubber material are significantly improved, which greatly expands the application field of rubber composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Transmission electron microscopy image of modified single-walled carbon nanotubes.
[0030] Figure 2 This is the Raman image of polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material.
[0031] Figure 3 Product picture of polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material. DETAILED DESCRIPTION
[0032] Hereinafter, an embodiment of an environmentally friendly rubber composite material of polydopamine / KH550 modified carbon nanotubes and a preparation method thereof of the present application will be specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0033] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0034] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0035] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0036] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0037] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0038] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0039] The invention provides an environmentally friendly rubber composite material of polydopamine and KH550 modified carbon nanotubes and a preparation method thereof. Single-walled carbon nanotubes are grafted and modified by polydopamine and KH550; the modified single-walled carbon nanotubes are added to a silicone rubber matrix to prepare a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material. Polydopamine is adsorbed on the surface of the single-walled carbon nanotubes through non-covalent π-π interactions, and its surface has certain active groups (such as -OH and -NH2), which creates an opportunity for secondary modification of the material. Then KH550 is grafted on the surface of polydopamine. Since its surface has many amino groups, the spacing between carbon nanotubes is increased, and hydrogen bonds can also be formed with substrate molecular chains, thereby improving the comprehensive performance of the composite material.
[0040] In one embodiment of the present application, the present application proposes a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material, comprising the following raw materials in parts by weight: 100 parts of silicone rubber, 2 to 8 parts of hydroxy silicone oil, 30 to 160 parts of carbon black, 0.5 to 2 parts of vulcanizing agent, 3 to 7 parts of silane coupling agent, 1 to 5 parts of single-walled carbon nanotubes, 1 to 5 parts of dopamine, and 1 to 5 parts of KH550.
[0041] The silane coupling agent is at least one of vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl tri(β-methoxyethoxy)silane, excluding KH550.
[0042] The hydroxy silicone oil is α,ω-dihydroxypolydimethylsiloxane with a dynamic viscosity of 30 to 40 mPa·s.
[0043] The vulcanizing agent is one of benzoyl peroxide, diisopropylbenzene peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0044] A method for preparing a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material comprises the following steps:
[0045] (1) Dispersing the single-walled carbon nanotubes uniformly in deionized water by ultrasonic oscillation, and adding a buffer solution to stabilize the pH of the single-walled carbon nanotube suspension within a certain range. Subsequently, a certain amount of dopamine is added to the solution, and after the room temperature deposition polymerization reaction is completed, washing, filtering, and drying are performed to obtain polydopamine-modified single-walled carbon nanotubes;
[0046] (2) After KH550 and deionized water are hydrolyzed in a three-necked flask under certain conditions, single-walled carbon nanotubes modified with polydopamine are added, and the reaction is continued. Finally, the single-walled carbon nanotubes with surface functionalization are obtained by filtering and drying.
[0047] (3) Weigh the corresponding weight of silicone rubber, silane coupling agent and hydroxy silicone oil, and stir them evenly in an internal mixer at high speed; add carbon black in batches and stir thoroughly after each addition; add the modified single-walled carbon nanotubes in batches and ensure that they are evenly mixed; when the temperature rises to 140-170°C, evacuate the mixture and stir for 1-3 hours to obtain a silicone rubber compound; after cooling to room temperature, add a vulcanizer on an open mixer and pass it through 3-5 times. After the colloid cools to room temperature, let it stand for more than 15 hours; and mold the compound at 140-160°C for 10-20 minutes and 10-20 MPa.
[0048] In some embodiments, the buffer solution used in step (1) is a tris(hydroxymethyl)aminomethane-hydrochloric acid mixed solution, and the pH range of the buffer solution is 5.5-8.
[0049] The tris-hydrochloric acid mixed solution has good stability, can maintain its buffering capacity, and is more conducive to dopamine in biomass; tris-hydrochloric acid and hydrochloric acid are both relatively low-toxic compounds and are relatively safe; the tris-hydrochloric acid mixed solution is easily soluble in water, and the preparation process is simple and does not require special operating skills; the prices of tris-hydrochloric acid and hydrochloric acid are relatively low, and the cost of preparing the Tris-HCl buffer solution is also relatively low.
[0050] In some embodiments, the deposition reaction time of dopamine in step (1) is 10 to 24 hours. The thickness of the dopamine deposition layer can be adjusted according to different deposition times.
[0051] The key is to precisely control the thickness of dopamine deposited on carbon nanotubes. Too thick a deposition thickness will result in: a. Reducing the electron mobility of carbon nanotubes: The electrical properties of carbon nanotubes, especially their carrier mobility, are crucial to their application as electronic devices (such as field effect transistors). Too thick a deposition of dopamine may inhibit the transmission of electrons in carbon nanotubes, thereby reducing mobility. b. Changing the morphology of carbon nanotubes: The deposition of dopamine may change the surface structure of carbon nanotubes, which may cause the wall of the tube to twist or deform, affecting its application in composite materials or catalysis. c. Inducing interfacial reactions: There is a chemical interaction between dopamine and carbon nanotubes, which may generate new interfacial compounds. Excessive deposition may induce chemical reactions at the interface, affecting the stability and performance of the material. d. Changes in catalytic performance: In catalytic applications, excessive deposition of dopamine may cover the active sites of carbon nanotubes, thereby reducing their catalytic efficiency. e. Reducing the mechanical strength of the material: Excessive deposition may increase the density of the material, thereby reducing its mechanical properties, especially in applications that require high mechanical strength. f. Influence on the biocompatibility of materials: In the biomedical field, the deposition of dopamine may affect the interaction between carbon nanotubes and biological tissues, thereby affecting their biocompatibility.
[0052] However, if dopamine is deposited too thinly on carbon nanotubes, it will cause: a. The functionalization effect is not obvious: the expected functionalization effect may not be effectively achieved. b. Reduced stability: the dopamine thin layer may not be sufficient to stabilize the surface functional groups of the carbon nanotubes, which reduces their stability under long-term use or specific environmental conditions, such as applications under high temperature or high humidity conditions. c. Changes in electrochemical properties: a dopamine layer that is too thin may not be able to effectively adjust the electrochemical properties of carbon nanotubes, such as capacitance or electron transport properties, which is crucial for applications such as electronic devices and supercapacitors. d. Reduced biocompatibility: In biomedical applications, a dopamine layer that is too thin may not provide sufficient biocompatibility, affecting the interaction between the material and the organism and the safety of the application.
[0053] The deposition reaction conditions of dopamine are as follows: the temperature is between room temperature and 50°C, and the pH is 5.5-8.
[0054] When the pH is too low, dopamine will exist in a neutral form, reducing the reaction activity; when the pH is too high, it may cause the instability of the solution; when the temperature is too low, the reaction rate is slow and the deposition is incomplete; when the temperature is too high, it may cause dopamine degradation or other side reactions.
[0055] In some embodiments, the ratio of the single-walled carbon nanotubes to dopamine used in step (1) is 1:1-3.
[0056] After extensive research, it was found that modified carbon nanotubes prepared within this ratio have the best performance. Too much dopamine may lead to excessive aggregation of dopamine molecules on the surface of carbon nanotubes, forming a thick and uneven coating. This will make the surface functionalized uneven and reduce the specific application performance of carbon nanotubes, such as electrochemical performance or biocompatibility. Too little dopamine may result in insufficient coverage of the carbon nanotube surface, or a thin dopamine layer. This will limit the chemical bonding between the dopamine functional groups and the carbon nanotubes, reduce the functionalization effect and stability, and thus affect its performance in various applications.
[0057] In some embodiments, in step (2), the mass ratio of KH560 to polydopamine-modified single-walled carbon nanotubes is 1 to 3, the reaction temperature is 40 to 60° C., and the reaction time is 3 to 6 hours.
[0058] Too much KH550 may cause the silane molecules to form a thick and uneven coating on the surface of the carbon nanotubes. In this case, the silane layer may not be able to fully bond with the surface of the carbon nanotubes, resulting in reduced stability and durability of the coating. In addition, too much silane layer will also affect the surface chemical properties of the carbon nanotubes, which may reduce their performance in specific applications.
[0059] Too little KH550 may result in insufficient silane modification on the surface of carbon nanotubes, or a thin modification layer. This will limit the chemical bonding between the silane groups and the carbon nanotubes, affecting the stability and functionalization of the coating. In some applications, there may be insufficient silane layer, resulting in unstable coating performance or failure to effectively protect the carbon nanotubes.
[0060] Too long a reaction time may cause KH550 to form an overly thick silane coating on the surface of carbon nanotubes, which will not only affect its binding force with carbon nanotubes, but may also cause degradation or denaturation of the polydopamine layer. In addition, a long reaction time may also cause unnecessary side reactions, resulting in the generation of impurities in the product, thus affecting the performance of the final material.
[0061] Insufficient reaction time may lead to insufficient bonding between KH550 and polydopamine-modified single-walled carbon nanotubes, resulting in a thin silane layer that cannot effectively improve the surface properties of carbon nanotubes, which may have a negative impact on subsequent functionalization and application effects, such as low bonding strength and poor stability.
[0062] Too high a reaction temperature may cause thermal degradation of some molecules of KH550 and polydopamine, resulting in a decrease in the quality of the reaction product. At the same time, at high temperatures, the accelerated reaction rate may lead to an unstable structure of the generated polymer chain, thus affecting the overall performance of the material.
[0063] Reaction temperature is too low:
[0064] If the reaction temperature is too low, the reaction rate will be slowed down, the combination efficiency of KH550 and polydopamine will be reduced, and the coating may be uneven or the combination is not strong, which will directly affect the surface modification effect and application performance of single-walled carbon nanotubes.
[0065] In some embodiments, the silicone rubber in step (3) is methyl vinyl silica gel with a molecular weight of 450,000 to 700,000, wherein the vinyl content is 0.1% to 3%; the mass ratio of the modified single-walled carbon nanotube to the silicone rubber is 1 to 10:100.
[0066] The above conditions are limited mainly to ensure that the final composite material has ideal performance and characteristics. If it is not within these ranges, it will lead to the following effects:
[0067] Too low molecular weight: may lead to insufficient mechanical properties of silicone rubber, such as decreased tear strength, abrasion resistance and pressure resistance.
[0068] Too high molecular weight: may cause the material to become too hard and brittle, reducing its flexibility and plasticity.
[0069] Lower than 1:100: If the amount of added single-walled carbon nanotubes is too low, it may not be possible to effectively improve the properties of silicone rubber, such as enhancing its mechanical properties or electrothermal properties.
[0070] Higher than 10:100: If the amount of added single-walled carbon nanotubes is too high, it may lead to increased material cost, poor processability, or aggregation, affecting the uniformity and stability of the composite material.
[0071] In some embodiments, the hydroxy silicone oil in step (3) is α,ω-dihydroxypolydimethylsiloxane, and has a dynamic viscosity of 30 to 40 mPa·s.
[0072] Selecting the right dynamic viscosity of silicone oil can ensure good lubrication and dispersibility in rubber. This helps to evenly disperse the silicone oil during the rubber mixing process, improve the stability and uniformity of the mixture, and thus affect the physical properties and quality of the final rubber product.
[0073] Appropriate dynamic viscosity can help silicone oil maintain appropriate fluidity and lubricity during rubber processing, which is beneficial to rubber extrusion, molding and processing. Too high or too low viscosity may cause problems in the processing process, such as poor dispersion, blockage or insufficient lubrication, affecting production efficiency and product quality.
[0074] In some embodiments, the silane coupling agent in step (3) is at least one of vinyl triethoxy silane, vinyl trimethoxy silane, and vinyl tri (β-methoxyethoxy) silane.
[0075] In some embodiments, the vulcanizing agent in step (3) is one of benzoyl peroxide, diisopropylbenzene peroxide, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0076] Example
[0077] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0078] Example 1
[0079] A method for preparing a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material, comprising the following steps:
[0080] (1) 1g of single-walled carbon nanotubes was uniformly dispersed in deionized water by ultrasonic oscillation, and a tris(hydroxymethyl)aminomethane-hydrochloric acid buffer solution with a pH of 7.5 was added. Subsequently, 1g of dopamine was added to the mixed solution, and the deposition polymerization reaction was carried out at room temperature for 24 hours. After completion, the suspension was vacuum filtered with a 0.22μm water-mixed fiber microporous filter membrane, the filter cake was washed with deionized water until neutral, and dried in an oven at 80°C for 12 hours to obtain polydopamine-modified single-walled carbon nanotubes.
[0081] (2) After 1g of KH-550 and deionized water were hydrolyzed in a three-necked flask under certain conditions, 1g of polydopamine-modified single-walled carbon nanotubes were added, and the mixture was stirred continuously at 40°C for 3h. Finally, the suspension was filtered with a 0.22μm filter membrane, and the filter cake was washed with deionized water and vacuum dried at 80°C for 12h to obtain surface functionalized single-walled carbon nanotubes;
[0082] (3) Weigh 100g of methyl vinyl silica gel, 3g of vinyl triethoxysilane and 2g of α,ω-dihydroxy polydimethylsiloxane, stir and mix them evenly in an internal mixer at high speed, then add 30g of carbon black in batches and stir thoroughly after each addition. Add 1g of surface functionalized single-walled carbon nanotubes in batches and ensure that they are evenly mixed. Vacuum and stir for 3h at 150℃ to obtain a silicone rubber compound. After the compound is cooled to room temperature, add 0.5g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and pass it through the open mixer 5 times. After standing for more than 15h, the compound is molded at 140℃ for 10min and 10MPa.
[0083] Example 2
[0084] A method for preparing a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material, comprising the following steps:
[0085] (1) 2 g of single-walled carbon nanotubes were uniformly dispersed in deionized water by ultrasonic oscillation, and a tris(hydroxymethyl)aminomethane-hydrochloric acid buffer solution with a pH of 7.5 was added. Subsequently, 2 g of dopamine was added to the mixed solution, and the deposition polymerization reaction was carried out at room temperature for 24 h. After completion, the suspension was vacuum filtered with a 0.22 μm water-mixed fiber microporous filter membrane, the filter cake was washed with deionized water until neutral, and dried in an oven at 80°C for 12 h to obtain polydopamine-modified single-walled carbon nanotubes.
[0086] (2) After 2 g of KH-550 and deionized water were hydrolyzed in a three-necked flask under certain conditions, 2 g of polydopamine-modified single-walled carbon nanotubes were added, and the mixture was stirred continuously at 40°C for 3 h. Finally, the suspension was filtered with a 0.22 μm filter membrane, and the filter cake was washed with deionized water and vacuum dried at 80°C for 12 h to obtain surface functionalized single-walled carbon nanotubes;
[0087] (3) Weigh 100g of methyl vinyl silica gel, 3g of vinyl triethoxysilane and 2g of α,ω-dihydroxy polydimethylsiloxane, stir and mix them evenly in an internal mixer at high speed, then add 30g of carbon black in batches and stir thoroughly after each addition. Add 2g of surface functionalized single-walled carbon nanotubes in batches and ensure that they are evenly mixed. Vacuum and stir for 3h at 150℃ to obtain a silicone rubber compound. After the temperature of the compound is cooled to room temperature, add 0.5g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and pass it through the open mixer 5 times. After standing for more than 15h, the compound is molded at 140℃ for 10min and 10MPa.
[0088] Example 3
[0089] A method for preparing a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material, comprising the following steps:
[0090] (1) 3 g of single-walled carbon nanotubes were uniformly dispersed in deionized water by ultrasonic oscillation, and a tris(hydroxymethyl)aminomethane-hydrochloric acid buffer solution with a pH of 7.5 was added. Subsequently, 3 g of dopamine was added to the mixed solution, and the deposition polymerization reaction was carried out at room temperature for 24 h. After completion, the suspension was vacuum filtered with a 0.22 μm water-mixed fiber microporous filter membrane, the filter cake was washed with deionized water until neutral, and dried in an oven at 80°C for 12 h to obtain polydopamine-modified single-walled carbon nanotubes.
[0091] (2) 3 g of KH-550 and deionized water were hydrolyzed in a three-necked flask under certain conditions, and then 3 g of polydopamine-modified single-walled carbon nanotubes were added. The mixture was stirred continuously at 40 °C for 3 h. Finally, the suspension was filtered with a 0.22 μm filter membrane, and the filter cake was washed with deionized water and vacuum dried at 80 °C for 12 h to obtain surface functionalized single-walled carbon nanotubes.
[0092] (3) Weigh 100g of methyl vinyl silica gel, 3g of vinyl triethoxysilane and 2g of α,ω-dihydroxy polydimethylsiloxane, stir and mix them evenly in an internal mixer at high speed, then add 30g of carbon black in batches and stir thoroughly after each addition. Add 3g of surface functionalized single-walled carbon nanotubes in batches and ensure that they are evenly mixed. Vacuum and stir for 3h at 150℃ to obtain a silicone rubber compound. After the temperature of the compound is cooled to room temperature, add 0.5g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and pass it through the open mixer 5 times. After standing for more than 15h, the compound is molded at 140℃ for 10min and 10MPa.
[0093] Example 4
[0094] A method for preparing a polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material, comprising the following steps:
[0095] (1) 5 g of single-walled carbon nanotubes were uniformly dispersed in deionized water by ultrasonic oscillation, and a tris(hydroxymethyl)aminomethane-hydrochloric acid buffer solution with a pH of 7.5 was added. Subsequently, 5 g of dopamine was added to the mixed solution, and the deposition polymerization reaction was carried out at room temperature for 24 h. After completion, the suspension was vacuum filtered with a 0.22 μm water-mixed fiber microporous filter membrane, the filter cake was washed with deionized water until neutral, and dried in an oven at 80°C for 12 h to obtain polydopamine-modified single-walled carbon nanotubes.
[0096] (2) After 5 g of KH-550 and deionized water were hydrolyzed in a three-necked flask under certain conditions, 5 g of polydopamine-modified single-walled carbon nanotubes were added, and the mixture was stirred continuously at 40 °C for 3 h. Finally, the suspension was filtered with a 0.22 μm filter membrane, and the filter cake was washed with deionized water and vacuum dried at 80 °C for 12 h to obtain surface functionalized single-walled carbon nanotubes;
[0097] (3) Weigh 100g of methyl vinyl silica gel, 3g of vinyl triethoxysilane and 2g of α,ω-dihydroxy polydimethylsiloxane, stir and mix them evenly in an internal mixer at high speed, then add 30g of carbon black in batches and stir thoroughly after each addition. Add 5g of surface functionalized single-walled carbon nanotubes in batches and ensure that they are evenly mixed. Vacuum and stir for 3h at 150℃ to obtain a silicone rubber compound. After the temperature of the compound is cooled to room temperature, add 0.5g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and pass it through the open mixer 5 times. After standing for more than 15h, the compound is molded at 140℃ for 10min and 10MPa.
[0098] Comparative Example 1
[0099] The steps for preparing the environmentally friendly rubber composite material are the same as those in Example 1, except that the amount of the surface functionalized single-walled carbon nanotubes added to the silicone rubber material is 10 g.
[0100] Comparative Example 2
[0101] The process of preparing the environmentally friendly rubber composite material is the same as step (3) of Example 1, except that 5 g of unmodified single-walled carbon nanotubes are added to the silicone rubber material.
[0102] Comparative Example 3
[0103] The process of preparing the environmentally friendly rubber composite material is the same as step (3) of Example 1, except that 5 g of multi-walled carbon nanotubes are added to the silicone rubber material.
[0104] Comparative Example 4
[0105] The process of preparing the environmentally friendly rubber composite material is the same as step (3) of Example 1, except that 5 g of graphene is added to the silicone rubber material.
[0106] Comparative Example 5
[0107] (1) 5 g of single-walled carbon nanotubes were uniformly dispersed in deionized water by ultrasonic oscillation, and a tris(hydroxymethyl)aminomethane-hydrochloric acid buffer solution with a pH of 7.5 was added. Subsequently, 5 g of dopamine was added to the mixed solution, and the deposition polymerization reaction was carried out at room temperature for 24 h. After completion, the suspension was vacuum filtered with a 0.22 μm water-mixed fiber microporous filter membrane, the filter cake was washed with deionized water until neutral, and dried in an oven at 80°C for 12 h to obtain polydopamine-modified single-walled carbon nanotubes.
[0108] (3) Weigh 100g of methyl vinyl silica gel, 3g of vinyl triethoxysilane and 2g of α,ω-dihydroxy polydimethylsiloxane, stir and mix them evenly in an internal mixer at high speed, then add 30g of carbon black in batches several times, and stir thoroughly after each addition. Add 5g of polydopamine-modified single-walled carbon nanotubes in batches and ensure that they are evenly mixed. Vacuum and stir for 3h at 150℃ to obtain a silicone rubber compound. After the temperature of the compound is cooled to room temperature, add 0.5g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and pass it through the open mixer 5 times. After standing for more than 15h, the compound is molded at 140℃ for 10min and 10MPa.
[0109] Comparative Example 6
[0110] (1) 5 g of KH-550 and deionized water were hydrolyzed in a three-necked flask under certain conditions, and then 5 g of single-walled carbon nanotubes were added. The mixture was stirred continuously at 40° C. for 3 h. Finally, the suspension was filtered with a 0.22 μm filter membrane, and the filter cake was washed with deionized water and vacuum dried at 80° C. for 12 h to obtain the modified single-walled carbon nanotubes.
[0111] (3) Weigh 100g of methyl vinyl silica gel, 3g of vinyl triethoxysilane and 2g of α,ω-dihydroxy polydimethylsiloxane, stir and mix them evenly in an internal mixer at high speed, then add 30g of carbon black in batches several times, and stir thoroughly after each addition. Add 5g of modified single-walled carbon nanotubes in batches and ensure that they are evenly mixed. Vacuum and stir for 3h at 150℃ to obtain silicone rubber compound. After the temperature of the compound is cooled to room temperature, add 0.5g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and pass it through the open mixer 5 times. After standing for more than 15h, the compound is molded at 140℃ for 10min and 10MPa.
[0112] The tensile strength and elongation at break of the polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material were tested. The experimental results are shown in Table 1.
[0113] Table 1
[0114]
[0115] It can be seen from Table 1 that the tensile strength and elongation at break of the silicone rubber composite materials of Examples 1-4 show a trend of increasing with the increase of the content of polydopamine / KH550 modified carbon nanotubes. This is because the interfacial compatibility of polydopamine / KH550 modified carbon nanotubes and silicone rubber in the composite material becomes stronger, the resulting interfacial adhesion increases to a certain extent, and the agglomeration phenomenon is reduced. The modified carbon nanotubes can effectively transfer the load during the stretching process, and the formation of hydrogen bonds may weaken the influence of stress concentration. In the silicone rubber composite material of Comparative Example 1, an excessive amount of polydopamine / KH550 modified carbon nanotubes is added, and the increase in filler content limits the movement of the molecular chain, resulting in poor tensile strength and elongation at break. In the silicone rubber composite material of Comparative Example 2, since the carbon nanotubes are not modified, the van der Waals force is large, resulting in serious agglomeration in the matrix, and the unmodified carbon nanotubes have poor compatibility with the silicone rubber matrix, and are prone to forming stress concentration points during the stretching process, which will cause the composite material to break prematurely, and the tensile strength and elongation at break are relatively low. The tensile strength and elongation at break of the silicone rubber materials of Comparative Examples 1 to 6 are worse than those of Example 4, indicating that the silicone rubber composite material prepared by the present invention has better mechanical properties.
[0116] The dielectric properties of the polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material were tested. The experimental results are shown in Table 2.
[0117] Table 2
[0118]
[0119] As can be seen from Table 2, with the increase of the content of polydopamine / KH550 modified carbon nanotubes, the dielectric constant of the composite material gradually increases and the dielectric loss gradually decreases. Since the interfacial interaction between KH550 and the polymer matrix promotes close bonding between each other, a conductive network will be formed in the silicone rubber, which improves the ability of silicone rubber to store charge and transfer electrons, thereby having better dielectric properties. In Comparative Example 1, the content of modified single-walled carbon nanotubes is too high, making it difficult to disperse evenly in the matrix and easy to agglomerate, resulting in an increase in the dielectric loss of the composite material. In Comparative Example 2, since the single-walled carbon nanotubes have not been modified, they are not compatible with silicone rubber and are easy to agglomerate in silicone rubber. They overlap each other to form a conductive path, and the space charge in the material moves in the path to generate leakage current, resulting in a large dielectric loss. The dielectric properties of Comparative Examples 1 to 6 are all worse than those of Example 4, indicating that the dielectric properties of the silicone rubber composite material of the present invention are better.
[0120] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A polydopamine / KH550 modified carbon nanotube environmentally friendly rubber composite material, It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of silicone rubber, 2-8 parts of hydroxy silicone oil, 30-160 parts of carbon black, 0.5-2 parts of vulcanizing agent, 3-7 parts of silane coupling agent, 1-5 parts of single-walled carbon nanotube, 1-5 parts of dopamine and 1-5 parts of KH550.
2. A method for preparing an environmentally friendly rubber composite material of polydopamine / KH550 modified carbon nanotubes, It is characterized in that The following steps are involved: (1) uniformly dispersing single-walled carbon nanotubes in deionized water, adding a certain amount of dopamine for deposition polymerization, and after the reaction is completed, washing, filtering, and drying to obtain polydopamine-modified single-walled carbon nanotubes; (2) After KH550 is hydrolyzed, single-walled carbon nanotubes modified with polydopamine are added, and after the reaction, the single-walled carbon nanotubes are filtered and dried to obtain surface functionalized single-walled carbon nanotubes; (3) Weigh corresponding weights of silicone rubber, silane coupling agent and hydroxy silicone oil, and mix them evenly in an internal mixer at high speed; add carbon black and the modified single-walled carbon nanotubes in (2) and mix them to obtain a silicone rubber compound. (4) After the silicone rubber mix has cooled, add the vulcanizer on the open mill, pass it through thinly, let the colloid stand for a period of time after it cools down, and finally perform compression molding.
3. The preparation method according to claim 2, It is characterized in that The specific steps include: (1) dispersing single-walled carbon nanotubes uniformly in deionized water by ultrasonic oscillation, and adding a buffer solution to stabilize the pH of the single-walled carbon nanotube suspension within a certain range; then, adding a certain amount of dopamine to the solution, and after the room temperature deposition polymerization reaction is completed, washing, filtering, and drying to obtain polydopamine-modified single-walled carbon nanotubes; (2) After KH550 and deionized water are hydrolyzed in a three-necked flask under certain conditions, single-walled carbon nanotubes modified with polydopamine are added, the reaction is continued, and finally, the single-walled carbon nanotubes with surface functionalization are obtained by filtering and drying; (3) Weighing corresponding weights of silicone rubber, silane coupling agent and hydroxy silicone oil, stirring and mixing them evenly in an internal mixer at high speed; adding carbon black in batches, stirring thoroughly after each addition; adding the modified single-walled carbon nanotubes in batches and ensuring that they are evenly mixed; When the temperature rises to 140-170°C, vacuum is applied and stirred for 1-3 hours to obtain a silicone rubber compound; (4) After cooling to room temperature, add vulcanizing agent on the open mill and pass it thinly for 3 to 5 times. After the colloid cools to room temperature, let it stand for more than 15 hours; the mixed rubber is molded at 140 to 160°C for 10 to 20 minutes and 10 to 20 MPa.
4. The preparation method according to claim 2, It is characterized in that The deposition reaction time of dopamine in step (1) is 10 to 24 hours. The thickness of the dopamine deposition layer can be adjusted according to different deposition times.
5. The preparation method according to claim 2, It is characterized in that The ratio of the single-walled carbon nanotubes to dopamine used in the step (1) is 1:1-3.
6. The preparation method according to claim 2, It is characterized in that In the step (2), the mass ratio of KH560 to the single-walled carbon nanotube modified with polydopamine is 1 to 3, the reaction temperature is 40 to 60° C., and the reaction time is 3 to 6 hours.
7. The preparation method according to claim 2, It is characterized in that The silicone rubber in step (3) has a molecular weight of 450,000 to 700,000 methyl vinyl silica gel, wherein the vinyl content is 0.1% to 3%; the mass ratio of the modified single-walled carbon nanotube to the silicone rubber is 1 to 10:
100.
8. The preparation method according to claim 2, It is characterized in that The hydroxy silicone oil in step (3) is a,ω-dihydroxypolydimethylsiloxane, and has a dynamic viscosity of 30 to 40 mPa.s.
9. The preparation method according to claim 2, It is characterized in that The silane coupling agent in step (3) is at least one of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tri (β-methoxyethoxy) silane.
10. The preparation method according to claim 2, It is characterized in that The vulcanizing agent in step (3) is one of benzoyl peroxide, diisopropylbenzene peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
Citation Information
Cited By
High-performance ethylene propylene diene monomer foaming material and preparation method thereof
CN119859355A
A preparation method of a degradable fiber composite material with synergistic enhancement of a nanoparticle-bimending interface
CN122706085A