Concentrated silicone defoaming emulsions

Through the preparation method of concentrated water-in-water silicone defoaming emulsion, the problems of increased viscosity and poor storage stability under high silicone concentration are solved, and a silicone defoaming agent with low viscosity, dispersible and high defoaming performance are achieved. Effectively inhibit foam formation.

CN119095917APending Publication Date: 2024-12-06ELKEM SILICONES FRANCE SAS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202380036848.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-03-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing silicone defoaming agents are prone to increase viscosity at high silicone concentrations, become difficult to handle and disperse, and have poor storage stability, affecting their availability and defoaming performance at the liquid-gas interface.

Method used

Using concentrated water-in-water silicone defoaming emulsion, the silicone defoaming agent, organopolysiloxane and emulsifier are dispersed at high temperatures, and water and additives are added during cooling to form a low viscosity, dispersible and stable storage. and the emulsion is added to the liquid surface to inhibit foam formation.

Benefits of technology

The silicone defoaming emulsion with low viscosity at high silicone concentration is achieved, maintaining good dispersion and storage stability, while improving the defoaming performance and simplifying the operation and transportation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005104857510000171
    Figure BDA0005104857510000171
  • Figure BDA0005104857510000181
    Figure BDA0005104857510000181
  • Figure BDA0005104857510000191
    Figure BDA0005104857510000191
Patent Text Reader

Abstract

The invention relates to a concentrated silicone-in-water defoaming emulsion, a preparation method and a method for inhibiting foam.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicone defoaming. More particularly, this invention relates to a concentrated water-in-water silicone defoaming emulsion that is workable, dispersible, storage-stable, and effective. The invention also relates to a method for preparing such a low-viscosity concentrated defoaming emulsion and a method for suppressing foam formation using such a concentrated defoaming emulsion. Background Art

[0002] Foam is a dispersion of air bubbles in a liquid or solid matrix. Surfactants or surface agents commonly used in various industries, such as detergents, wetting agents, emulsifiers, or dispersants, reduce the surface tension of liquids and, due to their amphiphilic nature, tend to accumulate at the gas-liquid interface, thus slowing down bubble coalescence and stabilizing the foam.

[0003] Defoaming compositions are systems that, when added to a foaming liquid, accelerate foam collapse relative to foam formation. Typically, these compositions are added at low concentrations. Defoamers have been found to be used in a variety of manufacturing and processing processes, such as paints and latexes, coating processes, textiles, fermentation processes, polymer manufacturing, cleaning compounds, pulp and paper, wastewater treatment, and cooling towers.

[0004] The addition of silicone defoaming compositions has proven particularly effective in controlling foam. Silicone defoaming compositions are dispersions of hydrophobic particles such as silica in a silicone matrix. US3383327 describes a composition comprising silica dispersed in polydimethylsiloxane and heated.

[0005] To achieve improved defoaming performance, polydimethylsiloxane can be partially replaced by three-dimensional networks or branched polymers.

[0006] For this purpose, EP0163541 describes a method for preparing a silicone defoamer by polycondensation reaction of a reactive organopolysiloxane having hydroxyl or alkoxy functional groups at a certain temperature in the presence of a catalyst, a silicone resin, a filler, and a non-reactive organopolysiloxane. Furthermore, EP2794760 describes a method for preparing a silicone defoamer at a certain temperature from a mixture of a reactive organopolysiloxane having hydroxyl functional groups, two types of silica (one hydrophobic and one hydrophilic), and an organosiloxane resin, respectively, in the presence of a catalyst. This also involves polycondensation reaction. Documents EP0434060, US8053480, and WO2021167728 describe silicone defoamers obtained by polyaddition chemistry. Patent applications WO2020108750 and 751 combine polyaddition and polycondensation chemistry. WO2021126195 also describes a chemistry involving irradiation using high-energy radiation.

[0007] However, these silicone defoamers can be viscous, which is detrimental to their use, and they are not easily dispersed in aqueous media. Furthermore, they sometimes exhibit viscoelastic behavior, also known as the Weissenberg effect. This effect is a manifestation of the non-zero normal stress difference typical of certain polymer solutions (viscoelastic fluids). This phenomenon manifests as the liquid rising along a rotating rod immersed in such a viscoelastic fluid. This is why they are formulated into water-in-water silicone emulsions with the addition of emulsifiers.

[0008] Various compositions for obtaining silicone defoaming emulsions have been described. For example, WO2016107987 describes a method for preparing silicone microdroplets in water, wherein the silicone content is limited to 10% by weight. Higher concentrations are described in WO1998000216, where examples consist of emulsions containing 35% solids. Emulsification of silicone defoamers typically requires the use of specific surfactants, such as the anhydrous sorbitol esters referenced in WO1998000216 and WO2016107987, which prevent the silicone defoamer from disrupting the interfacial layer of the emulsion.

[0009] For productivity and eco-design reasons, there is a growing desire to limit water concentration and therefore increase silicone concentration in silicone defoaming emulsions. However, it is well known in the emulsion industry that increasing the volume fraction of microdroplets leads to a significant increase in viscosity. By increasing the concentration, the emulsion evolves from a Newtonian state to a pseudoplastic non-Newtonian state and becomes extremely difficult to handle, pour, pump, and disperse.

[0010] In this context, on the one hand, there is a need for silicone defoaming emulsions with high viscosity or viscoelastic properties, which have a high silicone concentration while maintaining a low emulsion viscosity typically below 6000 mPa·s, preferably below 3500 mPa·s, and good storage stability. On the other hand, these emulsions can be dispersed in water to ensure the availability of the active component at the liquid-gas interface, which means that the defoaming performance must not be affected by the substances used for emulsification. Summary of the Invention

[0011] In this context, the present invention aims to satisfy at least one of the following objectives.

[0012] One object of the present invention is to provide an organosilicon defoaming emulsion that simultaneously meets the requirements of high organosilicon concentration, while maintaining low viscosity, dispersibility, storage stability and good defoaming performance.

[0013] Another fundamental objective of this invention is to provide a method for preparing a silicone defoaming emulsion, wherein the emulsion simultaneously meets the requirements of high silicone concentration, low viscosity, dispersibility, storage stability, and good defoaming performance.

[0014] Another fundamental objective of this invention is to provide a method for inhibiting foam formation using a silicone defoaming emulsion that is concentrated, low in viscosity, dispersible, storage stable, and has good defoaming properties.

[0015] Overview of the Invention

[0016] These and other objectives are achieved by the present invention, which primarily relates to a water-in-water silicone defoaming emulsion EA comprising:

[0017] - At least one first water-in-water silicone defoaming emulsion EA1, having a volume average diameter d EA1 For a thickness greater than or equal to 6 μm, the first water-in-water silicone defoaming emulsion EA1 contains:

[0018] a) At least one silicone defoamer AS, comprising 0.1-10% by weight of at least one mineral filler C,

[0019] b) Optionally, at least one organopolysiloxane B1,

[0020] c) At least one emulsifier D1

[0021] d) At least one additive F1,

[0022] e) Water W1, and

[0023] - At least one second water-in-water silicone emulsion E2, having a concentration less than d EA1 The average volume diameter d E2 The water-in-water silicone defoaming emulsion EA is characterized by containing less than 65% by weight, preferably less than 60% by weight, and more preferably less than 55% by weight of water.

[0024] This invention also relates to a method for preparing a water-in-water silicone defoaming emulsion EA, characterized in that the method comprises the following basic steps:

[0025] a) Disperse at least one silicone defoamer AS, optionally at least one organopolysiloxane B1, at least one emulsifier D1, and a portion of water under stirring and at a temperature above 50°C and below 75°C until the mixture is homogenized.

[0026] b) Cool the mixture obtained at the end of step a) with stirring until it reaches a temperature of less than or equal to 30°C, and add the second portion of water, followed by additive F1, and stir until the mixture is homogenized to obtain EA1.

[0027] c) Add water-in-water silicone emulsion E2 to EA1 and stir until the defoaming emulsion EA is completely homogenized.

[0028] The present invention also relates to a method for inhibiting foam formation by adding an antifoaming emulsion EA to the surface of a liquid.

[0029] Detailed instructions

[0030] This water-in-oil silicone defoaming emulsion EA contains:

[0031] - At least one first water-in-water silicone defoaming emulsion EA1, having a volume average diameter d EA1 For a thickness greater than or equal to 6 μm, the first water-in-water silicone defoaming emulsion EA1 contains:

[0032] a) At least one silicone defoamer AS, comprising 0.1-10% by weight of at least one mineral filler C,

[0033] b) Optionally, at least one organopolysiloxane B1,

[0034] c) At least one emulsifier D1

[0035] d) At least one additive F1,

[0036] e) Water W1, and

[0037] - At least one second water-in-water silicone emulsion E2, having a concentration less than d EA1 The average volume diameter d E2 The water-in-water silicone defoaming emulsion EA is characterized by containing less than 65% by weight, preferably less than 60% by weight, and more preferably less than 55% by weight of water.

[0038] The water-in-water silicone defoaming emulsion EA is characterized by having a viscosity of less than 6000 mPa·s, preferably less than 3500 mPa·s.

[0039] All viscosities considered in this disclosure correspond to the so-called “Newtonian” dynamic viscosity at 25°C, i.e., the dynamic viscosity measured in a manner known per se using a Brookfield viscometer at a sufficiently low shear rate gradient that makes the measured viscosity independent of the velocity gradient.

[0040] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the content of water-in-water silicone emulsion E2 is 2-30% relative to the total weight of water-in-water silicone defoaming emulsion EA, preferably 2.5-30% relative to the total weight of water-in-water silicone defoaming emulsion EA, more preferably 4-24%, and even more preferably 6-20%.

[0041] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the water-in-water silicone emulsion E2 has a volume average diameter d. E2 Emulsions with a thickness of 0.01-6 μm.

[0042] The average particle size was measured using laser particle size distribution. The average particle size corresponds to the diameter D[4,3], which is the volume average diameter. The definition of the volume average diameter D[4,3] is well known to those skilled in the art.

[0043] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the water-in-water silicone emulsion E2 is a water-in-water silicone emulsion with a silicone concentration greater than 35% by weight of the total weight of E2.

[0044] According to another preferred embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the water-in-water silicone emulsion E2 contains...

[0045] -35-80 parts by weight of at least one organopolysiloxane B2,

[0046] -0.1-10 parts by weight of at least one emulsifier D2,

[0047] -0-5 parts by weight of at least one additive F2, and

[0048] -5-65 parts by weight of water W2, for every 100 parts by weight of the sum of components B2, D2, F2 and W2.

[0049] The volume average diameter D[4,3] of emulsion EA1 is preferably greater than 6 μm, preferably 7-150 μm and even more preferably 10-120 μm.

[0050] To the volume average diameter d EA1 Adding volume average diameter d to water-in-silicone defoaming emulsion EA1 with a diameter greater than 6μm E2 Less than d EA1 The water-in-water silicone emulsion E2 allows for the simultaneous production of concentrated silicone emulsions and low viscosity. This results in increased productivity, ease of handling and transport, while maintaining good defoaming properties.

[0051] The water-in-water silicone defoaming emulsion EA according to the present invention simultaneously has a silicone content of more than 35%, a viscosity of less than 6000 mPa·s, preferably less than 3500 mPa·s, good dispersibility in water, good storage stability and good defoaming performance.

[0052] E2 is a water-in-water silicone emulsion based on organopolysiloxane.

[0053] To describe organopolysiloxanes, the silanoxy units M, D, T, and Q must be mentioned. The letter M represents the formula (R)3SiO. 1 / 2The monofunctional unit is where a silicon atom is bonded to a single oxygen atom in the polymer containing that unit. The letter D represents a difunctional unit where a silicon atom is bonded to two oxygen atoms (R)₂SiO₃. 2 / 2 The letter T represents the formula (R)SiO, where silicon atoms are bonded to three oxygen atoms. 3 / 2 The three functional units. The letter Q represents the SiO₂ formula where silicon atoms are bonded to four oxygen atoms. 4 / 2 The four functional units. The symbol R has the same characteristics as the symbol R defined below. 2 、R 3 and R 4 The same definition applies. Units M, D, and T can be functionalized. Therefore, when referring to units M, D, and T, the specific functional group should be specified.

[0054] Water-in-silicone emulsion E2 contains at least one organopolysiloxane B2, which may be selected from:

[0055] - A non-reactive organopolysiloxane, each molecule of which has monovalent organic substituents, which may be the same as or different from each other, attached to silicon atoms, and which are selected from C1-C1. 40 Alkyl, C3-C8 cycloalkyl, C6-C 10 Aryl and C7-C 50 Alkyl aryl;

[0056] -Reactive organopolysiloxanes containing at least two silanol groups ≡SiOH per molecule;

[0057] - and mixtures thereof.

[0058] Within the scope of this invention, the term "non-reactive" is understood to mean an organopolysiloxane that does not chemically react with any component of the emulsion under the conditions of emulsification, preparation and use of water-in-water silicone emulsions.

[0059] The non-reactive organopolysiloxane can be an oil or a glue, and preferably has a dynamic viscosity of 50-600,000 mPa·s at 25°C or a consistency of 200-2000 in tenths of a millimeter at 25°C.

[0060] The dynamic viscosity of the silicone was measured at 25°C according to ASTM D 445 standard.

[0061] The term "glue" is used for organopolysiloxane compounds with a viscosity typically greater than ~600,000 mPa·s, which corresponds to a molecular weight greater than 260,000 g / mol.

[0062] The consistency or penetration of the gel was determined at 25°C using a PNR12 penetration meter or an equivalent model that allows a cylindrical head to be applied to the sample under standardized conditions.

[0063] The penetration of the gel refers to the depth, expressed in tenths of a millimeter, that a calibrated cylinder penetrates into the sample in one minute.

[0064] For this purpose, the adhesive sample was introduced into an aluminum cup with a diameter of 40 mm and a height of 60 mm. A bronze or brass cylindrical head, with a diameter of 6.35 mm and a height of 4.76 mm, was carried by a 51 mm long and 3 mm diameter metal rod adapted to the penetration meter. This rod was weighted with an additional 100 g load. The total weight of the assembly was 151.8 g, of which 4.3 g was the cylindrical portion and its supporting rod. The cup containing the adhesive sample was placed in a constant temperature bath at 25 ± 0.5 °C for at least 30 minutes. Measurements were performed according to the manufacturer's instructions. The device displayed the depth (V) value in tenths of a millimeter and the time (t) to reach that depth in seconds. Penetration was equal to 60 V / t, expressed as tenths of a millimeter per minute.

[0065] The non-reactive organopolysiloxane adhesives available according to the present invention can be used alone or as a mixture in an inorganic solvent. The solvent may be selected from volatile organosilicones, octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), polydimethylsiloxane (PDMS) oil, polyphenylmethylsiloxane (PPMS) oil, or mixtures thereof, to avoid the use of organic solvents that are harmful to the environment and the health of workers in tire manufacturing plants.

[0066] Advantageously, the non-reactive organopolysiloxane is a linear non-reactive organopolysiloxane oil, which is a linear homopolymer or copolymer. Preferably, the linear non-reactive organopolysiloxane oil has a dynamic viscosity of about 0.65-100000 mPa·s at 25°C. As an example, the following linear organopolysiloxanes can be mentioned:

[0067] -Each chain consists of the following units:

[0068] i) Equation R 5 R 6 SiO 2 / 2 The unit, optionally with equation (R) 5 )2SiO 2 / 2 Unit combination,

[0069] ii) Formula (R) 6 )2SiO 2 / 2 The unit, optionally with equation (R) 5 )2SiO 2 / 2 Unit combination,

[0070] iii) Equation R 5 R 6 SiO 2 / 2unit and formula (R) 6 )2SiO 2 / 2 The unit, optionally with equation (R) 5 )2SiO 2 / 2 Unit combination,

[0071] -and at each end of the chain, by formula (R) 7 )3SiO 1 / 2 The unit end cap, where R 7 The groups are the same or different, selected from R 5 and R 6 group;

[0072] -wherein R is the monovalent organic substituent for the various silanoxy units mentioned above. 5 and R 6 A group has the following definition:

[0073] a)R 5 The groups may be the same or different from each other, selected from:

[0074] 1. Linear C1-C6 or branched C3-C6 alkyl groups, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, and

[0075] 2. C3-C8 cycloalkyl groups, such as cyclopentyl, cyclohexyl,

[0076] b)R 6 The groups may be the same or different from each other, selected from:

[0077] 1.C6-C 10 Aryl groups, such as phenyl, naphthyl,

[0078] 2.C7-C 15 Alkyl aryl groups, such as tolyl, xylyl, and

[0079] 3.C7-C 15 Arylalkyl groups, such as benzyl.

[0080] The reactive organopolysiloxane can be an oil or a glue, and preferably has a dynamic viscosity of 50-600,000 mPa·s at 25°C or a consistency of 200-2000 in tenths of a millimeter at 25°C.

[0081] Preferably, the reactive organopolysiloxane in the water-in-silicone emulsion E2 comprises the following silanoxy units:

[0082] M OH =[(OH)(R) 2 )2SiO 1 / 2 ]and D=[R3 R 4 SiO 2 / 2 ]

[0083] in:

[0084] R 2 、R 3 and R 4 It is selected from the following same or different groups:

[0085] -C1-C6 linear or branched alkyl groups, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl;

[0086] -C3-C8 cycloalkyl groups, such as cyclopentyl and cyclohexyl;

[0087] -C6-C 10 Aryl groups, such as phenyl and naphthyl groups; and

[0088] -C7-C 15 Alkyl aryl groups, such as tolyl and xylyl.

[0089] The water-in-silicone emulsion E2 also contains emulsifier D2. The properties of emulsifier D2 will be readily determined by those skilled in the art, with the aim of preparing a stable emulsion. Anionic, cationic, nonionic, and amphoteric surfactants can be used alone or in combination.

[0090] It should be noted that the water-in-silicone emulsion E2 may also contain a protective colloid such as polyvinyl alcohol, as described in patent EP0946240.

[0091] As anionic surfactants, the following surfactants can be mentioned:

[0092] -Form R a -CH(SO3M)-COOR b Alkyl ester sulfonates, wherein R a Indicates C8-C 20 C is preferred 10 -C 16 Alkyl, R b The expression indicates a C1-C6, preferably C1-C3 alkyl group, and M represents an alkali metal cation (sodium, potassium, lithium), substituted or unsubstituted ammonium (methylammonium, dimethylammonium, trimethylammonium, tetramethylammonium, dimethylpiperidine). Or derivatives of alkanolamines (monoethanolamine, diethanolamine, triethanolamine),

[0093] -Form R c Alkyl sulfates of OSO3M, wherein R c Indicate C 10 -C 24 C is preferred12 -C 20 Alkyl or hydroxyalkyl groups, where M represents a hydrogen atom or a cation having the same definition as above, and its ethoxide (OE) and / or propoxide (OP) derivatives, preferably having 1-20 OE units.

[0094] -Form R d CONHR e OSO3M alkylamide sulfate, wherein R d Indicates C2-C 22 C6-C is preferred. 20 Alkyl, R e The symbol represents a C2-C3 alkyl group, where M represents a hydrogen atom or a cation having the same definition as above, and its ethoxide (OE) and / or propoxide (OP) derivatives, preferably having 1-20 OE units.

[0095] -Saturated or unsaturated C8-C 24 C is preferred 14 -C 20 Salts of fatty acids, C9-C 20 Alkylbenzene sulfonates, and their ethoxide (OE) and / or propoxide (OP) derivatives, preferably having 1-20 OE units, -C9-C 20 Alkylbenzene sulfonates, primary or secondary C8-C 22 Alkyl sulfonates, alkyl glycerol sulfonates, sulfonated polycarboxylic acids (described in GB-A-1 082 179), alkyl sulfonates, N-acyl-N-alkyl taurines, monoalkyl and dialkyl phosphates, alkyl hydroxyethyl sulfonates, alkyl succinates, alkyl sulfosuccinates, sulfosuccinate monoesters or diesters, N-acyl sarcosinates, alkyl glycoside sulfates, polyethoxycarboxylates, cations that are alkali metals (sodium, potassium, lithium), substituted or unsubstituted ammonium residues (methylammonium, dimethylammonium, trimethylammonium, tetramethylammonium, dimethylpiperidine) Or derivatives of alkanolamines (monoethanolamine, diethanolamine, triethanolamine).

[0096] As nonionic surfactants, examples of poly(alkylene oxide) alkyl or aryl ethers include polyoxyethylene-modified sorbitan hexastearate, polyoxyethylene-modified sorbitan oleate, and poly(ethylene oxide) and cetyl stearyl ethers. Examples of poly(alkylene oxide) aryl ethers include polyoxyethylene-modified alkylphenol. Examples of poly(alkylene oxide) alkyl ethers include polyethylene glycol isodecanyl ether and polyethylene glycol trimethyl nonyl ether (each molecule contains 3-15 ethylene oxide units).

[0097] Examples of surfactants may also include: ionic, nonionic, or amphoteric fluorinated surfactants and mixtures thereof, such as:

[0098] - Perfluoroalkyl compounds,

[0099] -Perfluorobetaine,

[0100] -Ethoxylated polyfluorinated alcohol,

[0101] - Polyfluoroalkylammonium,

[0102] - wherein the hydrophilic portion comprises one or more sugar units having five to six carbon atoms and wherein the hydrophobic portion comprises formula R f (CH2) n - surfactants of unit n, where n = 2-20 and R f Expression C m F 2m+1 The perfluoroalkyl unit, wherein m = 1-10; and

[0103] - Polyelectrolytes with aliphatic perfluoroalkyl side groups.

[0104] The term "fluorinated surfactant" is understood to refer, as is entirely known in itself, to a compound consisting of an aliphatic perfluorocarbon moiety comprising at least three carbon atoms and an ionic, nonionic, or amphoteric hydrophilic moiety. The perfluorocarbon moiety having at least three carbon atoms may constitute all or only a portion of the fluorocarbon moiety of the molecule. Numerous references can be found in the literature regarding compounds of this type. Those skilled in the art may in particular refer to the following references:

[0105] -FR-A-2 149 519, WO-A-94 21 233, US-A-3,194,767, “Fluorinated Surfactants”, Erik Kissa, published by Marcel Dekker Inc., (1994), Chapter 4, especially Tables 4.1 and 4.4.

[0106] In particular, it is worth mentioning that the company Du Pont used the name Products sold, such as FSO, FSN-100, FS-300, FSD, and those sold by DU PONT under the name of... Fluorinated surfactants and those produced by 3M under the name Products for sale.

[0107] Among these surfactants, anionic, cationic, nonionic, and amphoteric perfluoroalkyl compounds deserve particular mention, and among them, those specifically named by DuPont are particularly noteworthy. FSA, FSO, FSC and FSK sales Class of surfactants.

[0108] The following can be further elaborated regarding them:

[0109] - FSO 100: CAS 65545-80-4, (non-ionic), 99%-100%, the remainder is 1,4-dioxanone. alkyl,

[0110] - FSN: CAS 65545-80-4, 99%-100%, the remainder is sodium acetate and 1,4-diethyl acetate. alkyl,

[0111] - FS-300: CAS 65545-80-4, 40%, the remainder is 1,4-2 Alkane (<0.1%) and water,

[0112] - FSD: CAS 70983-60-7, 30%, (cationic type), the remainder being hexanediol (10%), sodium chloride (3%) and water (57%).

[0113] You can also mention:

[0114] - Perfluoroalkyl betaine (amphoteric), for example, by DU PONT under the name Products sold under 1157 include ethoxylated polyfluorinated alcohols (nonionic type), such as those sold by DU PONT under the name FORAFAC 1110D, and polyfluoroalkyl ammonium salts (cationic type), such as those sold by DU PONT under the name FORAFAC 1179.

[0115] -The hydrophilic portion comprises one or more sugar units containing 5-6 carbon atoms (derived from fructose, glucose, mannose, galactose, tarol, gulolose, allose, altose, idole, arabinose, xylose, lysol, and / or ribose) and the hydrophobic portion comprises units of formula R F (CH2) n The unit (where n can be 2-20, preferably 2-10 and R) F Expression C m F 2m+1The surfactant is a perfluoroalkyl unit, wherein m can be 1-10, preferably 4-8), selected from those having the characteristics defined above; reference may be made to sugars such as sucrose and monoesters of perfluoroalkylated fatty acids, the monoester functional group being of formula R F (CH2) n C(O) represents, where n can be 2-10 and R F Expression C m F 2m+1 The perfluoroalkyl unit, wherein m can be 4-8; as described in the Journal of the American Association of Petroleum Chemists (JAOCS), Vol. 69, No. 1 (January 1992) and selected from those having the characteristics defined above; and

[0116] - Polyelectrolytes with aliphatic perfluoroalkyl side groups, such as those with R F (CH2) n Polyacrylates with groups, wherein n can be 2-20, preferably 2-10 and R F Expression C m F 2m+1 The perfluoroalkyl unit, wherein m can be 1-10, preferably 4-8; selected from those having the characteristics defined above; may be mentioned having -CH2C7F 15 Polyacrylates with the group as described in J. Chim. Phys. (1996) 93, 887-898 and selected from those having the characteristics defined above.

[0117] The amount of emulsifier D2 varies depending on the type of each component present and on the properties of the emulsifier itself. Typically, the emulsion contains 0.1% to 10% by weight of surfactant relative to the total weight of the emulsion.

[0118] Furthermore, additive F2, such as film-forming polymers, biocides, rheology modifiers, coalescing agents, dispersants, acidifiers, neutralizers, alkalis and / or thickeners, may be used in emulsions, either alone or as a mixture.

[0119] The concentration of such additives is known to those skilled in the art.

[0120] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the silicone defoamer AS is obtained through polycondensation chemistry.

[0121] The polycondensation chemistry is well known to those skilled in the art. Without limitation, references may be made to documents such as EP0163541 and EP2794760.

[0122] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the silicone defoamer AS is obtained through polyaddition chemistry.

[0123] The polyaddition or hydrogenation silanization chemistry is well known to those skilled in the art. Without limitation, references may be made to, for example, documents EP0434060, US8053480, WO2018224131, and WO2021167728.

[0124] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the silicone defoamer AS is obtained through free radical chemistry.

[0125] The free radical chemistry described is well known to those skilled in the art. Without limitation, references may be made to, for example, document WO2021126195.

[0126] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that the silicone defoamer AS is obtained by mixing different silicone defoamers AS.

[0127] The mineral filler C in the organosilicon defoamer AS is a compound selected from the following: silica, preferably combustion-processed silica and / or precipitated silica and / or colloidal silica, diatomaceous earth, ground quartz, calcium carbonate, hydrated alumina, magnesium hydroxide, carbon black, titanium dioxide, alumina, vermiculite, zinc oxide, mica, talc, iron oxide, barium sulfate, slaked lime, and mixtures thereof.

[0128] The mineral filler C in the organosilicon defoamer AS is preferably silica. It can be treated or untreated precipitated silica or combustion-processed silica. Precipitated silica is preferably pre-hydrophobicated by conventional treatment with one or more organosilicon compounds. It can be introduced untreated and then treated in situ (hydrophobicated) with one or more organosilicon compounds. Among these compounds, methylpolysiloxanes, such as hexamethyldisiloxane, octamethylcyclotetrasiloxane, methylpolysilazanes, such as hexamethyldisilazane, hexamethylcyclotrisilazane, chlorosilanes, such as dimethyldichlorosilane, trimethylchlorosilane, methylvinyldichlorosilane, dimethylvinylchlorosilane, and alkoxysilanes, such as dimethyldimethoxysilane, can be mentioned. During this treatment, the silica can increase its initial weight by up to 20%. Combustion-processed silica can be used untreated. However, if desired, it can be treated like precipitated silica.

[0129] Mineral packing material C typically has a minimum thickness of 10m as measured by the BET method. 2 / g, especially 20-300m 2 / g specific surface area.

[0130] A mixture of filler C can be used.

[0131] The content of mineral filler C is usually 0.1-10% by weight of silicone defoamer AS, preferably 0.5-10% by weight of silicone defoamer AS.

[0132] The silicone defoamer AS or the water-in-water silicone defoaming emulsion EA1 may optionally contain polyether silicone to improve defoaming performance. This polyether silicone is well known to those skilled in the art. For non-limiting purposes, references may be made to WO2020228212, EP3423165, EP2563491 and EP2563491.

[0133] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that it comprises water-in-water silicone defoaming emulsion EA1 with a water content of less than 65% by weight and water-in-water silicone emulsion E2 with a water content of less than 65% by weight.

[0134] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized by a bimodal particle size distribution of the dispersed oil phase, wherein the ratio of coarse particle percentage to fine particle percentage is between 98 / 2 and 60 / 40. The coarse particle percentage is calculated as the sum of (weight of silicone defoamer AS + weight of organopolysiloxane B1 + weight of emulsifier D1) of defoaming emulsion EA1 and (weight of (weight of silicone defoamer AS + weight of organopolysiloxane B1 + weight of emulsifier D1) of defoaming emulsion EA1 and the dry matter weight of emulsion E2), and the fine particle percentage is rounded up to 100%.

[0135] Preferably, the ratio of coarse particles to fine particles in the defoaming emulsion EA is between 98 / 2 and 70 / 30.

[0136] According to another embodiment, the water-in-water silicone defoaming emulsion EA is characterized in that it comprises, for 100 parts by weight of the defoaming emulsion EA:

[0137] -70-98 parts by weight of volume average diameter d EA1 A water-in-water silicone defoaming emulsion EA1 with a thickness greater than or equal to 6 μm, comprising:

[0138] a) 15-55 parts by weight of at least one silicone defoamer AS, which contains 0.1-10 parts by weight of at least one mineral filler C.

[0139] b) 0-25 parts by weight of at least one organopolysiloxane B1,

[0140] c) 0.1-12 parts by weight of at least one emulsifier D1,

[0141] d) 0.01-5 parts by weight of at least one additive F1,

[0142] e) 3-65 parts by weight of water W1, and

[0143] -2-30 parts by weight of at least one second water-in-silicone emulsion E2, which has a concentration of less than d EA1 The average volume diameter d E2 .

[0144] The organopolysiloxane B1 may be the same as or different from B2, and may be reactive or non-reactive as described for B2.

[0145] Emulsifier D1 may be the same as or different from D2. It can be a protective colloid such as polyvinyl alcohol or a nonionic, anionic, or cationic surfactant, used alone or in mixtures.

[0146] Additive F1 may be the same as or different from F2.

[0147] Another object of the present invention relates to a method for preparing a water-in-water silicone defoaming emulsion EA, characterized in that the method comprises the following basic steps:

[0148] a) Disperse at least one silicone defoamer AS, optionally at least one organopolysiloxane B1, at least one emulsifier D1, and a portion of water under stirring and at a temperature greater than 50°C and less than 75°C until the mixture is homogenized.

[0149] b) Cool the mixture obtained at the end of step a) with stirring until it reaches a temperature of less than or equal to 30°C, and add the second portion of water, followed by additive F1, and stir until the mixture is homogenized to obtain EA1.

[0150] c) Add water-in-water silicone emulsion E2 to EA1 and stir until the water-in-water silicone defoaming emulsion EA is completely homogenized.

[0151] More specifically, the present invention relates to a method for suppressing foam formation by adding a water-in-water silicone defoaming emulsion EA to the surface of a liquid. Detailed Implementation

[0152] Other advantages and features of the invention will become apparent from the following embodiments, which are given as non-limiting descriptions.

[0153] Example

[0154] In the following examples, different silicone defoamers AS, polydimethylsiloxane silicone oil B1, water-in-silicone emulsion E2, and emulsifier D1 were used to prepare the water-in-silicone defoaming emulsion EA according to the present invention. Unless otherwise stated, % is expressed as weight % throughout this document.

[0155] Raw materials used

[0156] Different commercial defoamers AS with a silica (C) content of 0.5-10% are used:

[0157] -Silcolapse TM 825, sold by Elkem Silicones, is an AS silicone defoamer obtained by polycondensation chemistry as described in EP0163541;

[0158] - 120, sold by Elkem Silicones, is an AS silicone defoamer as described in US3383327;

[0159] - 490, sold by Elkem Silicones, is an AS silicone defoamer obtained by polycondensation chemistry as described in EP0163541.

[0160] Bluesil TM FLD 47V350, sold by Elkem Silicones, is a non-reactive polydimethylsiloxane silicone oil B1 with a viscosity of ~350 mPa·s.

[0161] Bluesil TM FLD 48V135000, sold by Elkem Silicones, is a reactive (α,ω-dihydroxy) polydimethylsiloxane silicone oil B1 with a viscosity of ~135000 mPa·s.

[0162] Using different commercial emulsions E2:

[0163] Bluesil TM Emul 872, sold by Elkem Silicones, is an emulsion E2 of non-reactive polydimethylsiloxane silicone oil 47V350(B2) with ~61% dry matter and a volume average diameter D[4,3] of 0.16 μm.

[0164] -Bluesil Emul 284, from Elkem Silicones, is an emulsion E2 of reactive (α,ω-dihydroxy) polydimethylsiloxane silicone oil 48V135000 (B2) with ~51% dry matter and a volume average diameter D[4,3] of 0.26 μm.

[0165] Radiasurf 7145, sold by Oleon, is an emulsifier D1: sorbitan monostearate.

[0166] Myrj S40, marketed by Croda, is emulsifier D1: PEG-40 stearate.

[0167] Rhodasurf ROX, sold by Solvay, contains emulsifier D2: ethoxylated branched alcohol.

[0168] Proxel GXL, sold by Lonza, is Additive F1: a solution containing 20% ​​1,2-benzisothiazolin-3-one.

[0169] Characterization and Measurement Methods of Emulsions :

[0170] Dry extracts are expressed as % residue and measured using a halogen moisture analyzer (1 g - 105 ° C - 60 min).

[0171] The viscosity of the emulsion was measured initially and after one month at 40°C using a Brookfield viscometer (A4V20).

[0172] PSD particle size distribution was measured using a Malvern Mastersizer 3000 Laser Granulometer. D[4,3] corresponds to the volume-average diameter, expressed in μm.

[0173] The ease of use of the emulsion was estimated by filtering it through a 250 μm nylon sieve.

[0174] To estimate the dispersibility of the emulsion, drops of emulsion were pipetted into a cylindrical tube 4.5 cm high and 1.4 cm in diameter filled with 3 ml of deionized water. The number of complete inversions required for complete dispersion was quantified. If the number of complete inversions was less than 10, preferably less than 5, the emulsion was considered dispersible.

[0175] Regarding storage stability, a visual inspection is performed every two months. The number of months following the observation of phase separation is recorded.

[0176] Defoaming performance was checked using a recirculation test. 800 ml of detergent solution (containing 3 g / L sodium dodecylbenzenesulfonate and an aqueous solution of C12-C18 fatty alcohols ethoxylated seven times on average) was pumped into a 2 L test tube at a flow rate of 200 L / h at 60 °C. Once the foam level reached the H1 scale (in ml), 50 mg of defoaming emulsion was injected, and the foam level was monitored over time. Initially, as the foam level decreased, its lowest point (H2 in ml) was recorded, allowing the calculation of the "effect" (1 - (H2 / H1)) as a percentage.

[0177] Composition and properties of emulsion EA obtained by a single silicone defoamer AS.

[0178] [Table 1]

[0179] Composition (g) of antifoaming emulsion EA Comparative Example 1 According to Embodiment 1 of the present invention Defoaming emulsion EA1 Silcolapse 825 (Silicone Defoamer AS) 155 154 Bluesil 47V350 (Silicone Oil B1) 210 110 Radiasurf 7145 (Emulsifier D1) 66.9 49.5 Myrj S40 (Emulsifier D1) 23 16.6 Water W1 442 394 Proxel GXL (Additive F1) 1.4 1.4 Bluesil Emul 872(E2) 0 176 Total weight EA (g) 898.3 901.5 % coarse particles 100 75 % fine particles 25 characteristic PSD type Single peak Twin Peaks D[4,3]μm 90 54 Initial viscosity A4V20 (mPa.s) >10 000 270 Extract % 51 48 Filtered through a 250μm sieve no yes Dispersibility in water (number of flips) >20 1 Viscosity A4V20 (mPa.s) after 1 month at 40℃ >10 000 1410 Phase separation after x months 4 months >12 months

[0180] According to Embodiment 1 of the present invention In a glass container equipped with a stirring anchor, add 154g of Silcolapse 825AS, 110g of Bluesil 47V350 B1, 49.5g of Radiasurf 7145D1, 16.6g of Myrj S40 D1, and 65.1g of deionized water W1 (Part 1). Stir at 60 rpm for 45 minutes while heating to 65°C to melt the emulsifier and homogenize the mixture. Then increase the stirring speed to 150 rpm and maintain for 20 minutes. Afterward, cool the mixture to 30°C, and at this temperature, add 329g of deionized water W1 (Part 2) at 10 rpm over one hour while continuing to cool to ambient temperature. Increase the stirring speed to 50 rpm and maintain for 25 minutes. Then add 176g of Bluesil Emul 872 Emulsion E2 over 15 minutes. Finally, add 1.4g of Proxel GXL F1 and continue stirring for 15 minutes.

[0181] The obtained concentrated water-in-water silicone defoaming emulsion is a white emulsion with a bimodal particle size distribution, a volume average diameter D[(4,3)] of 54 μm, a dry extract content of 48%, and a viscosity of 270 mPa·s, which is ~37 times lower than that of Comparative Example 1, which has a comparable dry extract content.

[0182] Unlike Comparative Example 1, the emulsion also passed through a 250 μm sieve without problems and was dispersible. Its viscosity after one month at 40°C was well below 3500 mPa·s.

[0183] Comparative Example 1 The experiment was conducted according to Example 1 (the difference being the addition of Bluesil Emul 872 emulsion E2), using the amounts of each ingredient mentioned in Table 1. In the absence of Bluesil Emul 872 emulsion E2, the resulting emulsion exhibited a unimodal particle size distribution, a volume-average diameter [D(4,3)] of ~90 μm, and a viscosity greater than 10,000 mPa·s, which is for a dry extract equivalent to that of Example 1 according to the invention. Unlike Example 1 according to the invention, the emulsion could not pass through a 250 μm sieve, exhibited poor dispersibility, and a phase shift was observed after 4 months.

[0184] Composition and properties of emulsion EA obtained from a mixture of two silicone defoamers AS.

[0185] [Table 2]

[0186]

[0187]

[0188] According to embodiments 2-5 of the present invention The procedure was carried out according to Example 1, using the amounts of each component mentioned in Table 2. A mixture of two silicone defoamers AS was used instead of just one silicone defoamer AS. A white emulsion was obtained with a bimodal particle size distribution, a volume average diameter [D(4,3)] between 34 and 13 μm, and a viscosity of less than 6000 mPa·s for approximately 50% dry extract, i.e., a viscosity 2-10 times lower than that of Comparative Example 2 at a comparable dry extract. All emulsions passed through a 250 μm sieve, exhibited good dispersibility (less than or equal to 5 tumbles), and a viscosity of less than 6000 mPa·s after one month at 40°C. No phase separation was observed after 12 months of storage, while good defoaming performance was observed: the measured impact effect was greater than 89%.

[0189] Comparative Example 2 The experiment was conducted according to Examples 2-5 (the difference being the addition of emulsion E2 in Examples 2-5), using the amounts of each ingredient mentioned in Table 2. The resulting emulsion was a very viscous white paste exhibiting a unimodal particle size distribution. The volume-average diameter was ~70 μm, and the viscosity was greater than 10,000 mPa·s for the dry extract equivalent to that of Examples 2-5 according to the invention. Unlike Examples 2-5 according to the invention, this emulsion could not pass through a 250 μm sieve, exhibited poor dispersibility (>20 tumbles), and phase separation was observed after 6 months.

[0190] Composition and properties of emulsion EA obtained from emulsion E2 with different average volume diameters.

[0191] [Table 3]

[0192]

[0193] Preparation of E2 emulsion :

[0194] Bluesil Emulsion 284: E2 D[4,3]=3.5μm

[0195] 195 g of Bluesil FLD 48V135000 oil B2, 16.1 g of Rhodasurf ROX D2, and 6.5 g of deionized water W2 (part 1) were placed in a glass container equipped with a stirring anchor. The mixture was stirred at 30 rpm for 20 minutes, followed by the addition of 134 g of deionized water W2 (part 2) over 15 minutes. Once all the water had been incorporated, stirring was maintained at 100 rpm for 15 minutes, and 0.5 g of Proxel GXL F2 was added. The resulting water-in-silicone oil emulsion was a white emulsion with a volume average diameter [D(4,3)] of 3.5 μm and a dry extract content of 58.5%.

[0196] Bluesil Emulsion 284: E2 D[4,3]=5.5μm

[0197] 177 g of Bluesil FLD 48V135000 oil B2, 9.6 g of Rhodasurf ROX D2, and 9.0 g of deionized water W2 (part 1) were placed in a glass container equipped with a stirring anchor. The mixture was stirred at 40 rpm for 10 minutes, followed by the addition of 157 g of deionized water W2 (part 2) over 20 minutes. Once all the water had been incorporated, stirring was maintained at 100 rpm for 15 minutes, and 0.5 g of Proxel GXL F2 was added. The resulting water-in-silicone oil emulsion was a white emulsion with a volume average diameter [D(4,3)] of 5.5 μm and a dry extract content of 51.6%.

[0198] According to embodiments 6-9 of the present invention The experiment was conducted according to Example 1, using the amounts of each component mentioned in Table 3. Emulsion E2 with different volume average diameters was used. A white emulsion with a bimodal particle size distribution and a volume average diameter [D(4,3)] of 12.3–4.5 μm was obtained, with a viscosity of less than 6000 mPa·s for approximately 66% dry extract, i.e., a viscosity 2–7 times lower than that of Comparative Example 3 at a comparable dry extract. All emulsions passed through a 250 μm sieve, exhibited good dispersibility (less than or equal to 5 tumbles), and a viscosity of less than 6000 mPa·s after one month at 40°C.

[0199] Comparative Example 3 The experiment was conducted according to Examples 6-9 (the difference being the addition of emulsion E2 in Examples 6-9), using the amounts of each ingredient mentioned in Table 3. The resulting emulsion was a viscous white paste exhibiting a unimodal particle size distribution. The volume-average diameter was ~70 μm, and the viscosity was 9950 mPa·s for a dry extract equivalent to that of Examples 6-9 according to the invention. Unlike Examples 6-9 according to the invention, this emulsion could not pass through a 250 μm sieve and exhibited poor dispersibility (9 flips).

Claims

1. Water-in-organic silicone defoaming emulsion EA, the water-in-organic silicone defoaming emulsion EA comprises: - at least one first silicone-in-water antifoam emulsion EA1 having a volume average diameter d EA1 is greater than or equal to 6 μm, and the first water-in-water silicone defoaming emulsion EA1 comprises: a) at least one silicone defoamer AS comprising 0.1 to 10% by weight of at least one mineral filler C, b) optionally, at least one organopolysiloxane B1, c) at least one emulsifier D1, d) at least one additive F1, e) water W1, and - at least one second silicone-in-water emulsion E2 having a content of less than d EA1 The volume average diameter d E2 , and is characterized in that the silicone-in-water antifoam emulsion EA contains a water content of less than 65% by weight.

2. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: It has a viscosity of less than 6000 mPa.s.

3. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: The content of the silicone-in-water emulsion E2 is 2-30% relative to the total weight of the silicone-in-water antifoaming emulsion EA.

4. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: The volume average diameter d of water-in-silicone emulsion E2 is E2 It is an emulsion of 0.01-6μm.

5. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: The silicone-in-water emulsion E2 is a silicone-in-water emulsion having a silicone concentration greater than or equal to 35% by weight of the total weight of E2.

6. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: Water-in-silicone emulsion E2 contains - 35 to 80 parts by weight of at least one organopolysiloxane B2, - 0.1 to 10 parts by weight of at least one emulsifier D2, - 0 to 5 parts by weight of at least one additive F2, and 5 to 65 parts by weight of water W2 per 100 parts by weight of the sum of components B2, D2, F2 and W2.

7. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: Silicone defoamers AS are obtained via polycondensation chemistry.

8. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: Silicone defoamers AS are obtained via polyaddition chemistry.

9. The silicone-in-water defoaming emulsion EA according to claim 1, characterized in that: Silicone defoamers AS are obtained via free radical chemistry.

10. The silicone-in-water defoaming emulsion EA according to claim 1, characterized in that: The organosilicon defoamer AS is obtained by mixing different organosilicon defoamers AS.

11. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: It comprises a water-in-organic silicone defoaming emulsion EA1 having a water content of less than 65% and a water-in-organic silicone emulsion E2 having a water content of less than 65%.

12. The water-in-silicone defoaming emulsion EA according to claim 1, characterized in that: The particle size distribution of the dispersed oil phase is bimodal, with a ratio of coarse particle percentage / fine particle percentage between 98 / 2 and 60 / 40, the coarse particle percentage being calculated as follows: the sum of (the weight of silicone antifoam AS + the weight of organopolysiloxane B1 + the weight of emulsifier D1) of the antifoam emulsion EA1 / (the weight of (the weight of silicone antifoam AS + the weight of organopolysiloxane B1 + the weight of emulsifier D1) of the antifoam emulsion EA1 and the dry matter weight of emulsion E2), and the fine particle percentage being made up to 100%.

13. The water-in-silicone defoaming emulsion EA according to any one of claims 1 to 12, characterized in that: It comprises, for 100 parts by weight of antifoam emulsion EA: -70-98 parts by weight of volume average diameter d EA1 The water-in-organic silicone defoaming emulsion EA1 is greater than or equal to 6 μm, and the water-in-organic silicone defoaming emulsion EA1 comprises: a) 15 to 55 parts by weight of at least one silicone defoamer AS containing 0.1 to 10 parts by weight of at least one mineral filler C, b) 0 to 25 parts by weight of at least one organopolysiloxane B1, c) 0.1 to 12 parts by weight of at least one emulsifier D1, d) 0.01 to 5 parts by weight of at least one additive F1, e) 3-65 parts by weight of water W1, and - 2 to 30 parts by weight of at least one second silicone-in-water emulsion E2 having a d EA1 The volume average diameter d E2 .

14. A method for preparing the water-in-silicone defoaming emulsion EA according to claim 1, characterized in that The method includes the following basic steps: a) dispersing at least one silicone defoamer AS, optionally at least one organopolysiloxane B1, at least one emulsifier D1 and a portion of the water under stirring and at a temperature of greater than 50° C. and less than 75° C. until the mixture is homogenous, b) cooling the mixture obtained at the end of step a) with stirring until a temperature less than or equal to 30° C. and adding a second portion of water and then the additive F1 and stirring until the mixture is homogenous, to obtain EA1, c) Add water-in-silicone emulsion E2 to EA1 and stir until the water-in-silicone defoaming emulsion EA is completely homogenized.

15. A method for inhibiting foam formation by adding water-in-silicone defoaming emulsion EA to the surface of a liquid, characterized in that The silicone-in-water defoaming emulsion EA is the silicone-in-water defoaming emulsion EA according to claims 1 to 13 or the silicone-in-water defoaming emulsion EA obtained according to claim 14.

Citation Information

Cited By

  • Efficient organic silicon defoaming agent suitable for metal working fluid as well as preparation method and application of efficient organic silicon defoaming agent

    CN119588034A

  • High-efficiency silicone defoamer applicable to metalworking fluids, its preparation method and application

    CN119588034B