Thick-wall pipeline steel coil tower shape control method
By controlling the temperature uniformity and deviation value during heating and rolling, combined with dynamic side guide control and auxiliary roll pressure boost, the tower shape exceeds the standard caused by cold sickle bending of thick-walled pipeline steel is solved, and the system is significantly improved Pass rate.
Patent Information
- Application Number
- CN202411320007.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Thick-walled pipeline steel is prone to cold sickle bending defects during rolling and coiling, resulting in the steel coil shape exceeding the standard, affecting production efficiency and pipe-controlling pass rate.
By controlling the temperature difference between the two sides of the slab during heating, the deviation value of the head of the outlet strip and the center line of the rough and fine rolling process is defined, and a two-way strong side spray device and dynamic side guide pressure are used during the strong cooling process after rolling. Position control, correct the bending direction of the sickle on the head of the steel belt, and adopts the pressure boost control mode of the auxiliary roller.
The thickness of the steel coil tower and the correction rate of thick-walled pipelines have been significantly reduced, and the pipe passing rate has been improved, and the improvement of sickle bending has reached more than 85%.
Smart Images

Figure CN119114644A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a tower shape control method for a thick-wall pipeline steel coil. Background Art
[0002] With the continuous improvement of the national oil and gas pipeline network's requirements for pipeline transportation capacity and efficiency, pipeline steel has been developing towards high strength and large wall thickness in recent years. X70~X90 with a thickness of more than 17.5mm has become the mainstream trend of the high-grade pipeline steel market. These requirements of downstream users have posed new challenges to high-grade pipeline steel coils based on hot rolling production lines. First, in order to meet the demand for high strength, pipeline steel must use a strong cooling system after rolling to cool the temperature to the bainite transformation zone below 500℃ to meet the performance requirements. However, this temperature range is in the transient boiling zone, and the cooling uniformity is poor, which makes the strip steel very prone to post-cold sickle bending defects, resulting in excessive tower shape of the steel coil after coiling. Secondly, due to the large thickness, the unit length of the strip steel is heavy, the centering and correction ability of the guide plate on the front side of the coiling is weak, and the poor centering leads to the tower shape of the steel coil. Thirdly, due to the characteristics of large wall thickness and high strength, the strip head is difficult to form during the coiling process and is easy to displace and shift, causing the inner ring to bulge, forming a tower defect.
[0003] For pipeline steel coils, downstream pipe-making enterprises mainly roll the steel coils into spirals at a certain angle using rollers and weld them into steel pipes after the steel coils are put on line. However, due to the problem of excessive tower shape, the steel coils cannot be put on line, or the tower-shaped steel coils are difficult to center after unrolling, affecting the production efficiency of users. Therefore, users cannot use the steel coils with excessive tower shape or it is difficult to use them, causing losses to the enterprises. Summary of the invention
[0004] The purpose of the present invention is to provide a method for controlling the tower shape of a thick-walled pipeline steel coil, reduce the degree of sickle bending of the strip head, significantly reduce the tower shape value and tower shape modification rate of the thick-walled pipeline steel coil, and improve the user's pipe manufacturing qualification rate.
[0005] The technical solution adopted by the present invention is: A method for controlling the tower shape of a thick-walled pipeline steel coil comprises the following steps: Step 1, after the billet is heated to the target temperature T1 in the heating furnace, it is rolled out of the furnace, and the temperature difference between the operation side and the transmission side of the billet out of the furnace is ≤30°C; Step 2, the steel billet is subjected to rough rolling, and the difference between the actual position of the head of the rough rolling outlet billet and the center line offset is ≤20mm; Step 3, the steel billet is subjected to finish rolling, and the difference between the actual position of the head of the strip at the finish rolling exit and the center line offset is ≤40mm; Step 4, the steel billet is strongly cooled after rolling to form a steel strip for coiling; According to the sickle bending direction of the head of the cold steel strip, the pressure control and position control method of the side guide plate of the coiler are dynamically used to correct the feeding direction of the head of the steel strip; The head of the steel coil adopts the auxiliary roll pressure boost control mode; Coiled into steel coils for shipment.
[0006] Preferably, before step 1, the method further includes the following steps: smelting and casting into steel billets according to the chemical composition.
[0007] Preferably, in step 1, T1 is 1170-1210°C. Preferably, in step 4, the water pressure for strong cooling after piercing is 2.5-3.0 bar.
[0008] Preferably, in step 4, the temperature of the steel strip during coiling is CT 300-450°C. Preferably, two-way strong side spray devices are provided on both sides of the steel strip. When the steel strip is coiled, the two-way strong side spray devices are turned on at the same time to remove the disorderly flowing water film on the surface of the steel strip.
[0009] Preferably, the strong side spray pressure of the bidirectional strong side spray device is ≥30KN.
[0010] Preferably, in the step 4, in the auxiliary winding roller pressure boost control mode adopted at the head of the steel coil, the pressure of the auxiliary winding roller for the first three turns is respectively increased by 8-12%, 5-8% and 2-5% compared with the original design pressure.
[0011] The original design pressure was 501KN, and the pressure increase gradually decreased according to the number of coiling turns. For example, for 18.5mm*1500mm X80 pipeline steel, the original auxiliary coiling roller design pressure was 501KN, and the pressure was set to 561KN (increased by 12%) in the first turn, 541KN (increased by 8%) in the second turn, and 526KN (increased by 5%) in the third turn.
[0012] In the step 4, the specific process of dynamically correcting the feeding direction of the steel strip head according to the sickle bend direction of the steel strip head after cooling is as follows: according to the sickle bend direction of the steel strip head after cooling, dynamically select the guide plate on the coiler side to correct the feeding direction of the steel strip head through pressure control and position control.
[0013] Preferably, when the sickle bending direction of the head of the cold steel strip is the transmission side, the side guide plate on the transmission side is controlled by position, and the side guide plate on the working side is controlled by pressure to correct the feeding direction of the head of the steel strip; When the sickle bending direction of the head of the cold steel strip is the working side, the side guide plate on the transmission side is controlled by pressure, and the side guide plate on the working side is controlled by position to correct the feeding direction of the head of the steel strip.
[0014] When the side guide plate adopts pressure control, the side guide plate moves and squeezes toward the transportation center line to ensure that the strip is in close contact with the side guide plate before coiling. When the side guide plate adopts position control, it ensures that the head of the strip is aligned with the reel before coiling and does not deviate.
[0015] Taking the case where the sickle bend direction of the incoming material head is the transmission side, at this time, the side guide plate on the transmission side is selected for position control, the maximum pressure of the side guide plate can reach 80KN, and the position does not change; and the side guide plate on the working side is selected for pressure control, which can play the function of correcting the deviation of the side guide plate when the center of the rear steel belt is biased toward the working side and the pressure surges, while ensuring that the side guide plate on the working side will not be fully opened due to excessive pressure. The beneficial effects of the present invention are: The present invention controls the temperature difference between the two sides of the slab to be ≤30°C during the heating process, thereby achieving cross-sectional temperature uniformity control during the rolling process from the source; controls the influence of sickle camber during the rolling process by limiting the deviation value between the head and the center line of the strip at the outlet of the rough and fine rolling processes; reduces the degree of sickle camber at the head of the strip, greatly reduces the tower shape value and the tower shape modification rate of the thick-walled pipeline steel coil, and improves the user's pipe manufacturing qualification rate due to the simultaneous improvement of the sickle camber. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the control method when the strip head is coiled with a sickle bend biased toward the transmission side in an embodiment of the present invention.
[0017] In the figure: 1-strip head; 2-operating side guide plate; 3-driving side guide plate; 4-operating side guide plate in a pressure-controlled manner; 5-driving side guide plate in a position-controlled manner; 6-reel. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0019] In the description of the present invention, it should be understood that if the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like are involved, the orientation or position relationship indicated is based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0020] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection. It can be a mechanical connection or an electrical connection. It can be directly connected or indirectly connected through an intermediate medium. It can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0021] Example 1 A method for controlling the tower shape of a thick-walled pipeline steel coil, the implementation steps are as follows: 1) Smelting and casting into steel billets according to the chemical composition; 2) After the billet is heated to the target temperature of 1170~1210℃ in the heating furnace, it is rolled out of the furnace. The temperature difference between the operation side and the transmission side of the billet out of the furnace is ≤30℃; 3) The billet is rough rolled, and the difference between the actual position of the billet head at the rough rolling exit and the center line offset is ≤20mm; 4) The steel billet is subjected to finish rolling, and the difference between the actual position of the billet head at the finish rolling exit and the center line offset is ≤40mm; 5) The billet is strongly cooled after rolling, the water pressure is 2.5~3.0bar, the coiling temperature CT is 300~450℃, and the two-way strong side spray device is turned on at the same time. The side spray pressure is ≥30KN, and the device is used to remove the disorderly flowing water film on the surface of the strip; 6) According to the sickle bending direction of the head of the cold steel strip, dynamically select the pressure control and position control mode of the coiling side guide plate to correct the steel feeding direction of the head of the steel strip; 7) The coil head adopts the auxiliary roll pressure boost control mode: the pressure of the auxiliary roll in the first three circles is increased by 8~12%, 5~8% and 2~5% respectively compared with the original design pressure; 8) Coil the steel into coils for shipment.
[0022] The original design pressure was 501KN, and the pressure increase gradually decreased according to the number of coiling turns. For example, for 18.5mm*1500mm X80 pipeline steel, the original auxiliary coiling roller design pressure was 501KN, and the pressure was set to 561KN (increased by 12%) in the first turn, 541KN (increased by 8%) in the second turn, and 526KN (increased by 5%) in the third turn.
[0023] The specific process of dynamically correcting the feeding direction of the steel strip head according to the sickle bend direction of the steel strip head after cooling is as follows: according to the sickle bend direction of the steel strip head after cooling, the guide plate on the coiler side is dynamically selected to correct the feeding direction of the steel strip head through pressure control and position control.
[0024] Furthermore, when the sickle bending direction of the head of the cold steel strip is the transmission side, the side guide plate on the transmission side is controlled by position, and the side guide plate on the working side is controlled by pressure to correct the feeding direction of the head of the steel strip; When the sickle bending direction of the head of the cold steel strip is the working side, the side guide plate on the transmission side is controlled by pressure, and the side guide plate on the working side is controlled by position to correct the feeding direction of the head of the steel strip.
[0025] When the side guide plate adopts pressure control, the side guide plate moves and squeezes toward the transportation center line to ensure that the strip is in close contact with the side guide plate before coiling. When the side guide plate adopts position control, it ensures that the head of the strip is aligned with the reel before coiling and does not deviate.
[0026] like Figure 1 As shown, taking the direction of the sickle bend of the incoming material head as the transmission side as an example, at this time, the side guide plate on the transmission side is selected for position control, the maximum pressure of the side guide plate can reach 80KN, and the position does not change; and the side guide plate on the working side is selected for pressure control, which can play the function of correcting the deviation of the side guide plate when the center of the rear steel belt deviates to the working side and the pressure surges, while ensuring that the side guide plate on the working side will not be fully opened due to excessive pressure.
[0027] The key process parameter values and implementation effect verification of the embodiments of the present invention are shown in the following table; Table 1 List of main process parameter values of the embodiments of the present invention;
[0028] Table 1 is a list of main process parameter values of the embodiments of the present invention;
[0029] Table 2 Implementation effect verification of the embodiments of the present invention
[0030] In summary, the present invention aims at the main factors causing the thick-walled pipeline steel tower type and innovates the process control points: 1) The sickle bend at the head of the strip is one of the main factors causing the tower-shaped defect: The present invention has carried out technological innovations on the factors that cause sickle bend in the production process of thick-walled pipeline steel. By controlling the temperature difference on both sides of the slab to ≤30°C during the heating process, the cross-sectional temperature uniformity control of the rolling process is achieved from the source. Secondly, the influence of sickle bend during the rolling process is controlled by limiting the deviation value between the head of the strip and the center line at the outlet of the rough and fine rolling process. Thirdly, by optimizing the control of the water volume on the upper and lower surfaces of the strip and the movement of residual water on the upper plate during low-temperature cooling, uniform cooling of the cross-section of the strip during the cooling process is achieved, and the degree of sickle bend at the head of the strip is reduced.
[0031] 2) In order to solve the problem of sickle bend before coiling, a method combining pressure control and position control of the coiling side guide plate is invented to dynamically select the direction of sickle bend. In this way, when the steel coil has sickle bend before coiling, the side guide plate can prevent it from running off, thus ensuring the stability of the coiling process. In order to solve the problem that the head of the steel coil is unstable and easy to deviate when entering the coiler, a pressure setting mode for the auxiliary winding roller at the coiling head was invented. By increasing the pressure of the auxiliary winding roller in the three circles of the head, the accurate coiling and forming of the steel coil head is ensured.
[0032] The present invention has the following advantages: 1) the maximum value of the steel coil tower shape of thick-walled pipeline steel is reduced from 100 mm to within 40 mm; 2) the steel coil tower shape correction rate is reduced from 4.45% to 0.68%, with a reduction of more than 85%; 3) due to the synchronous improvement of the sickle bend, the user's pipe manufacturing qualification rate increases by 0.5%.
[0033] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0034] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A method for controlling the tower shape of a thick-walled pipeline steel coil, characterized in that: The following steps are involved: Step 1, after the billet is heated to the target temperature T1 in the heating furnace, it is rolled out of the furnace, and the temperature difference between the operation side and the transmission side of the billet out of the furnace is ≤30°C; Step 2, the steel billet is subjected to rough rolling, and the difference between the actual position of the head of the rough rolling outlet billet and the center line offset is ≤20mm; Step 3, the steel billet is subjected to finish rolling, and the difference between the actual position of the head of the strip at the finish rolling exit and the center line offset is ≤40mm; Step 4, the steel billet is strongly cooled after rolling to form a steel strip for coiling; According to the sickle bending direction of the steel strip head after cooling, dynamically correct the steel strip head feeding direction; The head of the steel coil adopts the auxiliary roll pressure boost control mode; Coiled into steel coils.
2. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 1, characterized in that: Before step 1, the method further includes the following steps: smelting and casting into steel billets according to the chemical composition.
3. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 1, characterized in that: In the step 1, T1 is 1170-1210°C.
4. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 1, characterized in that: In step 4, the water pressure for strong cooling after piercing is 2.5-3.0 bar.
5. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 1, characterized in that: In step 4, the temperature of the steel strip during coiling is 300-450°C.
6. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 5, characterized in that: Two-way powerful side spray devices are installed on both sides of the steel strip. When the steel strip is coiled, the two-way powerful side spray devices are turned on at the same time to remove the disorderly flowing water film on the surface of the strip.
7. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 6, characterized in that: The powerful side spray pressure of the bidirectional powerful side spray device is ≥30KN.
8. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 1, characterized in that: In the step 4, in the auxiliary winding roller pressure boost control mode at the head of the steel coil, the auxiliary winding roller pressures of the first three turns are respectively increased by 8-12%, 5-8%, and 2-5% compared with the original design pressure.
9. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 1, characterized in that: In the step 4, the specific process of dynamically correcting the feeding direction of the steel strip head according to the sickle bend direction of the steel strip head after cooling is as follows: according to the sickle bend direction of the steel strip head after cooling, dynamically select the guide plate on the coiler side to correct the feeding direction of the steel strip head through pressure control and position control.
10. The method for controlling the tower shape of a thick-walled pipeline steel coil according to claim 9, characterized in that: When the sickle bending direction of the head of the cold steel strip is the transmission side, the side guide plate on the transmission side is controlled by position, and the side guide plate on the working side is controlled by pressure to correct the feeding direction of the head of the steel strip; When the sickle bending direction of the head of the cold steel strip is the working side, the side guide plate on the transmission side is controlled by pressure, and the side guide plate on the working side is controlled by position to correct the feeding direction of the head of the steel strip.
Citation Information
Patent Citations
Method for improving camber of intermediate slab in rough rolling
CN102319741A
Low-temperature coiling method for thick X120 pipeline steel hot rolled coils
CN102962296A
Method for correcting deviation of side guide plates of coilers
CN109127733A
Hot continuous rolling production method of thick-specification X70 pipeline steel strip coil
CN111330974A
Hot-rolled large-wall-thickness high-grade pipeline steel coil shape control method
CN112845611A
Cited By
Method for improving bending forming quality of head of steel plate
CN121696272A