Method for obtaining Brinell hardness of ductile material

By constructing a small punch test model of ball pressing and plane loading head, using power index and hardening coefficient to predict the Brinell hardness of the material, the problems of cumbersome measurement and unstable results in the prior art are solved, and efficient and accurate fabrics are achieved 1.5.5.5.6.6.6.6.6.6.6.6.6.6.6.

CN119124901APending Publication Date: 2024-12-13NAT ENERGY LARGE-SCALE PHYSICAL ENERGY STORAGE TECH R&D CENT IN BIJIE HIGH-TECH IND DEV ZONE +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174112.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-13

AI Technical Summary

Technical Problem

The method for obtaining the hardness of the material Brinell in the prior art has the problem of cumbersome measurement of the indentation area, unstable results, and irreversible damage to the service structure. The model stability of the elastic-plastic semi-analysis method is poor, so it is impossible to obtain the material Brinell efficiently and conveniently. hardness.

Method used

By constructing the small punch test load P-displacement h model of the ball pressing model and the plane loading head, combined with the definition of Brinell hardness, the Brinell hardness prediction model is constructed using parameters such as power index and strain hardening coefficient K and strain hardening index n. , perform power law fitting to obtain the strain hardening coefficient and index of the material, thereby predicting the Brinell hardness of the material.

Benefits of technology

It realizes Brinell hardness acquisition without measuring indentation size, stable results, high accuracy and strong universality, overcomes the uplift and sinking effects and irreversible damage problems of traditional hardness tests, and is suitable for energy storage containers, aerospace and Nuclear power and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119124901A_ABST
    Figure CN119124901A_ABST
Patent Text Reader

Abstract

The invention discloses a method for obtaining the Brinell hardness of a ductile material, and relates to a mechanical property testing technology of the ductile material. The method for obtaining the Brinell hardness of the ductile material is based on the equivalence of the energy density of the material in a complex stress state and the energy density of the material in a uniaxial stress state. And constructing a ball press-in model for describing the relationship of the sample load P-displacement h under the loading of the ball loading head, a small punch test load P-displacement h model for describing the relationship of the sample load P-displacement h under the loading of the small punch of the plane loading head, and a Brinell hardness prediction model for obtaining the Brinell hardness of the to-be-tested structural material. The method solves the problems that in the practical application process of a conventional method, the measurement result is greatly influenced by a measurement tool and a tester, sampling can cause irreversible damage to a service structure, and a semi-analytical method is poor in model stability for the Brinell hardness of a material influenced by the pile-up and sink-in effects, so that the measurement result is difficult to test, and the like. And the prediction accuracy cannot be ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a mechanical property testing technology of a ductile material, and in particular to a method for obtaining the Brinell hardness of a ductile material. Background Art

[0002] Structures serving in physical energy storage, aerospace, nuclear power and other environments, such as pressure vessels, will suffer varying degrees of structural damage and changes in mechanical properties due to their structural materials serving under harsh conditions such as high pressure and corrosion for a long time. Obtaining the Brinell hardness of the serving structural materials is an important part of evaluating the safety of the material structure.

[0003] In the process of realizing the present invention, the inventors found that there are at least the following problems in the prior art: At present, the methods for obtaining the Brinell hardness of materials at home and abroad mainly include the definition method and the elastoplastic semi-analytical method.

[0004] (1) Definition: GB / T 231.1-2018 "Brinell hardness test for metallic materials - Part 1: Test method" applies a specified load F to a cemented carbide ball of a certain diameter. B Press into the sample surface, and after a specified holding time, remove the load F B , by measuring the load F B The ratio of the residual indentation area to the Brinell hardness is used to characterize the Brinell hardness, and the corresponding relationship is given, namely:

[0005]

[0006] In the formula, the area of ​​the residual indentation for different types of materials (steel or aluminum) needs to be measured separately. In actual application, it is more troublesome, and the measurement results are greatly affected by the measuring tools and testers. It is difficult to obtain the Brinell hardness of the test material stably and accurately, and sampling will cause irreversible damage to the service structure.

[0007] (2) Elastic-plastic semi-analytical method: The semi-analytical prediction model of the Brinell hardness of the material is obtained through the Hollomon law parameters of the material, that is,

[0008]

[0009] In the above formula, K and n are the material hardening coefficient and strain hardening exponent respectively, and k1, k2, k3 and k4 are model constants, which can be determined by finite element analysis. The elastic recovery depth h is determined by the semi-analytical equation of the above formula with the help of the complete load P-displacement h curve. e , residual depth h r and predicted elastic segment depth h e0The Brinell hardness of the material is thus solved. However, for the Brinell hardness of materials affected by pile-up and sink-in effects, the model has poor stability and the accuracy of the prediction cannot be guaranteed. Summary of the invention

[0010] The purpose of the present invention is to provide a method for obtaining the Brinell hardness of a ductile material with little damage to the material of a service container and good stability, thereby overcoming the difficulty that the existing Brinell hardness test requires measuring the indentation area each time and cannot efficiently and conveniently obtain the Brinell hardness of the material.

[0011] To achieve this purpose, on the one hand, a method for obtaining the Brinell hardness of a ductile material is provided, the method for obtaining the Brinell hardness of a ductile material comprising the following steps:

[0012] Step 1: Based on the equivalence between the energy density of the material under complex stress state and the energy density of the material under uniaxial stress state, a ball indentation model describing the relationship between the load P and the displacement h of the specimen under ball loading is constructed; the ball indentation model uses the power exponent m B , parameter P * , the material's strain hardening coefficient K, strain hardening exponent n and the first set of model constants k1-k4 are described;

[0013] Step 2: Based on the equivalence between the energy density of the material under the complex stress state and the energy density of the material under the uniaxial stress state, a small punch test load P-displacement h model of the plane loading head is constructed to describe the relationship between the load P and the displacement h of the specimen under the loading of the small punch of the plane loading head; the small punch test load P-displacement h model of the plane loading head uses the power exponent m, the parameter P * , the strain hardening coefficient K, the strain hardening exponent n and a second set of model constants k5-k8;

[0014] Step 3: According to the definition of Brinell hardness, a Brinell hardness prediction model for obtaining the Brinell hardness of the structural material to be tested is constructed in combination with the ball indentation model and the small punch test load P-displacement h model of the plane loading head;

[0015] Step 4: prepare a circular thin sheet sample of the same material as the structure to be tested, perform a quasi-static test of a small punch of a plane loading head on the circular thin sheet sample, and obtain a load P-displacement h curve of the circular thin sheet sample;

[0016] Step 5: Take the data of the specified section of the load P-displacement h curve of the circular thin sheet sample, perform power law fitting according to the load P-displacement h model of the small punch test of the plane loading head, and obtain the strain hardening coefficient K and strain hardening exponent n of the material;

[0017] Step 6: Substitute the material strain hardening coefficient K and strain hardening exponent n obtained in step 5 into the Brinell hardness prediction model to obtain the Brinell hardness prediction value of the material to be tested.

[0018] Further, the ball pressing model is:

[0019]

[0020] Where P * is the characteristic load, P is the specified load, m B is the power index, n B is a given value, K is the strain hardening coefficient, D is the diameter of the ball in the ball indentation test, and h is the depth of ball indentation.

[0021] Furthermore, the small punch test load P-displacement h model of the planar loading head is:

[0022]

[0023] Where B is the sample thickness, d is the punch diameter, and m is the power exponent.

[0024] Furthermore, the Brinell hardness prediction model is:

[0025]

[0026] The above formula HBW is the Brinell hardness, α i is the third set of model constants, η is given by the standard.

[0027] Furthermore, the third set of model constants is obtained through the small punch test of the planar loading head in step four.

[0028] Furthermore, the first group of model constants k1-k4 and the second group of model constants k5-k8 are calibrated and obtained respectively through finite element analysis.

[0029] Furthermore, a testing system suitable for physical energy storage pressure vessels.

[0030] Furthermore, the invention is applicable to a test system for aerospace equipment.

[0031] Furthermore, the invention is applicable to a test system of nuclear power equipment.

[0032] One of the above technical solutions has the following advantages or beneficial effects:

[0033] The method of obtaining the Brinell hardness of ductile materials in this scheme overcomes the dilemma that the existing Brinell hardness test needs to measure the indentation area each time and cannot efficiently and conveniently obtain the Brinell hardness of the material, and fills the gap in the traditional small punch test to obtain the Brinell hardness of the material.

[0034] This method for obtaining the Brinell hardness of ductile materials uses a very small sample size, does not need to measure the indentation size, and has stable results, high accuracy, and strong universality. It solves the problems of large deviations in the indentation size measurement of materials with pile-up and sink-in effects in traditional hardness tests, irreversible damage to in-service pressure vessels caused by sampling, and inconsistent measurement results from different measuring instruments.

[0035] At the same time, the method for obtaining the Brinell hardness of elastic materials in this scheme adopts a new loading method of a planar loading head, so that the load P-displacement h curve is simple and highly stable, and the Brinell hardness of ductile materials can be obtained efficiently, universally and accurately, which is of great significance for obtaining the Brinell hardness of ductile materials that are widely used in key engineering fields such as energy storage containers, aerospace, and nuclear power. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is the step of obtaining the Brinell hardness of the ductile material in the first embodiment;

[0037] Figure 2 is a schematic diagram of the ball penetration test;

[0038] Figure 3 yes Figure 2 The load P-displacement h curve of the test specimen loaded to the specified load;

[0039] Figure 4 It is a schematic diagram of the small punch test device with a flat loading head. DETAILED DESCRIPTION

[0040] In order to make the technical problems solved by the present invention, the technical solutions adopted and the technical effects achieved clearer, the technical solutions of the embodiments of the present invention will be further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0041] In the description of the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0042] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0043] Embodiment 1:

[0044] like Figure 1 As shown, the method for obtaining the Brinell hardness of a ductile material in this embodiment includes the following steps:

[0045] S1: Based on the equivalence between the energy density of materials under complex stress states and that under uniaxial stress states, a ball indentation model is constructed to describe the load P-displacement h relationship of the specimen under ball loading.

[0046] The ball indentation model uses the power index m B , parameter P*, material strain hardening coefficient K, strain hardening exponent n and the first set of model constants k1-k4, the ball indentation test under ball loading head loading and the construction process of the ball indentation model are as follows:

[0047] Figure 2 A schematic diagram showing the ball penetration test, Figure 3 The load P-displacement h curve diagram of the specimen under the ball indentation test is shown. In the diagram, D is the ball diameter, P is the specified load, which is 1835N, and h is the indentation depth.

[0048] For metal materials that meet the requirements of continuity, uniformity, and isotropy, this paper uses the Hollomon law to describe the equivalent stress-strain relationship of the material, that is,

[0049]

[0050] Where E is the elastic modulus of the material. y and ε y are the nominal yield strength and nominal yield strain, ε y =σ y / E;σ eq and ε eq are the equivalent stress and equivalent strain, K and n are the strain hardening coefficient and strain hardening exponent, respectively.

[0051] Assume that there is a geometric point M in the representative volume unit of the material continuously distributed within the effective deformation domain Ω of the specimen. The energy density u of the RVE at point M is M is the average energy density in Ω, that is

[0052]

[0053] In the formula, ε ij and σ ij is the strain tensor and stress tensor of the RVE at point M, ε ij-M is the strain tensor of RVE at point M under a specific deformation state; V eff is the effective deformation volume of Ω; U is the total deformation energy in the effective deformation domain, expressed as

[0054]

[0055] Assume that the RVE energy density at point M under complex stress state is equivalent to the RVE energy density under uniaxial equivalent stress state, that is,

[0056]

[0057] In the formula, ε eq-M is the equivalent strain of RVE at point M under a specific deformation state.

[0058] According to equations (2) and (4), the total deformation energy U within the specimen deformation domain Ω can be expressed as

[0059]

[0060] Substituting equation (1) into equation (5), we can obtain

[0061]

[0062] Due to the obvious stress concentration at the tip of the indenter, the local material is in a high strain state. eq-M Much larger than ε y , compared to can be ignored, then formula (6) can be simplified to

[0063]

[0064] Assume V eff and ε eq-M There is a power law relationship between the dimensionless displacement h / d and

[0065]

[0066] Where k1 and k2 are the effective volume coefficient and effective volume index, respectively, and k3 and k4 are the effective strain coefficient and effective strain index, respectively.* is the feature depth, V * is the characteristic volume, and V * =A * h * , A * is the characteristic area, where h * =D,A * =πD 2 / 4.

[0067] During the ball indentation test, the material loading position satisfies the following relationship

[0068]

[0069] Under quasi-static loading conditions, the work done by the external force W is equal to the total deformation energy U in the compressive deformation area, that is,

[0070]

[0071] Taking the derivative of both sides of equation (10) with respect to U by h, and combining equations (8) and (9), we can get

[0072]

[0073] Where P is the specified load, h is the penetration depth, and the first set of model constants k1~k4 can be calibrated by finite element analysis calculation of a small number of working conditions. When calibrating k1~k4, the strain hardening exponent n B is a given value. Depending on the material, n B The value is 0.1 to 0.3, with an interval of 0.05. The first set of model constants after calibration is given in Table 1.

[0074] Table 1 Ball indentation test model constants

[0075]

[0076] S2: Based on the equivalence between the energy density of materials under complex stress states and the energy density of materials under uniaxial stress states, a small punch test load P-displacement h model of a plane loading head is constructed to describe the relationship between the load P and the displacement h of the specimen under the small punch loading of the plane loading head. The small punch test load P-displacement h model of a plane loading head is described using the power exponent m, the parameter P*, the strain hardening coefficient K, the strain hardening exponent n, and a second set of model constants k5-k8.

[0077] The construction process of the load P-displacement h model of the small punch test of the plane loading head is:

[0078] The uniaxial stress-strain relationship of most metals or alloys (aluminum alloys, magnesium alloys, titanium alloys, etc.) conforms well to the Hollomon power law hardening model, that is, it satisfies

[0079]

[0080] Where E is the elastic modulus, σ y is the nominal yield stress and n is the strain hardening exponent.

[0081] For the small punch test with a plane loading head, the following relationship is satisfied between the geometric dimensions of the small punch specimen, the material constitutive relationship parameters, displacement and load through theoretical derivation, that is, the load P-displacement h model of the small punch test with a plane loading head

[0082]

[0083] Where P * is the characteristic load, m is the loading index, B is the disc specimen thickness, and d is the punching diameter. The second set of model constants k5~k8 can also be calibrated by finite element analysis calculation of a small number of working conditions. When calibrating k5~k8, the strain hardening exponent n B is a given value. Depending on the material, n B The second set of model constants is given in Table 2.

[0084] Table 2 Model constants of small punch test with flat loading head

[0085]

[0086] At the same time, the yield strain ε y The correction of loading index m is as follows:

[0087] m t =c0+c1m+c2ε y (14)

[0088] m t In order to correct the loading index of the load P-displacement h curve, the parameters c0, c1, and c2 in the correction formula are listed in Table 3.

[0089] Table 3 Model correction constants

[0090]

[0091] S3: According to the definition of Brinell hardness, a Brinell hardness prediction model for obtaining the Brinell hardness of a material is constructed by combining the ball indentation model and the small punch test load P-displacement h model of a plane loading head, as follows:

[0092] When characterizing the Brinell hardness of a material, it is found that the following relationship exists between the ball indenter diameter D, the load P and the indentation diameter d:

[0093] P=Kπd 2 (d / D) n(15)

[0094] Where k and n (1>n>0) are material constants

[0095] GB / T 231.1-2018 "Brinell hardness test for metallic materials - Part 1: Test method" defines the Brinell hardness and stipulates that under load P, the total indentation depth h can be divided into the elastic recovery depth h e and plastic depth h p ,Right now

[0096] h=h e +h p (16)

[0097] The depth h of the elastic section of the existing ball indentation load P-displacement h curve e The formula predicts that

[0098]

[0099] In the formula, υ and E are the Poisson’s ratio and elastic modulus of the compressive material, respectively.

[0100] According to GB / T 231.1-2018 "Brinell hardness test for metallic materials - Part 1: Test method", D, d and indentation plastic depth h in the Brinell hardness test are p The following relationship exists:

[0101]

[0102] Substituting equation (18) into equation (15), we have

[0103]

[0104] GB / T 231.1-2018 "Brinell hardness test for metallic materials - Part 1: Test method" gives the definition of Brinell hardness, namely

[0105]

[0106] In the formula, η is a constant given by GB / T 231.1-2018 standard and its value is 0.102.

[0107] Substitute equation (19) into equation (20), and combine equations (17) and (11), and consider the effect of m on HBW t Make corrections, that is

[0108]

[0109] Formula (21) is the Brinell hardness prediction model for the structural material to be tested.

[0110] The first group of model constants k1~k4 are shown in Table 1, and the second group of model constants k5~k8 are shown in Table 2. i is the third set of model constants.

[0111] S4: Make a circular thin sheet sample with the same material as the structure to be tested, and perform a quasi-static test of a small punch with a flat loading head on the circular thin sheet sample to obtain the load P-displacement h curve of the circular thin sheet sample. The quasi-static test process of the small punch refers to GB / T231.1-2018 "Brinell hardness test of metallic materials Part 1: Test method".

[0112] Figure 4 This is a schematic diagram of a small punch test with a flat loading head. The material of the circular thin sample in the figure is the same as the material of the structure to be tested. The quasi-static test with a small punch with a flat loading head consists of a thin circular sample clamped by upper and lower clamps. The middle normal is the diameter d f The cylinder with a diameter of 1 mm is loaded. r is the chamfer radius of the lower fixture, which is 0.2 mm, d is the aperture of the lower fixture, which is 4 mm, B is the thickness of the disc sample, which is 0.5 mm, and D is the sample diameter, which is 10 mm.

[0113] S5: Take the data of the specified segment of the load P-displacement h curve of the circular thin slice specimen, perform power law fitting according to the load P-displacement h model of the small punch test with a flat loading head, and obtain the strain hardening coefficient K and strain hardening exponent n of the material. The specific process is as follows:

[0114] Take the data of the h∈{0.15~0.3} segment of the load P-displacement h curve, and fit the data of the h∈{0.15~0.3} segment according to formula (13). In the formula, according to the test in step S4, d is the aperture of the lower fixture, which is 4 mm, B is the thickness of the disc sample, which is 0.5 mm, and D is the sample diameter, which is 10 mm. Substitute them into the second set of model constants k5~k8 obtained in Table 2. The strain hardening coefficient K and strain hardening exponent n of the corresponding material can be obtained through formula (13).

[0115] The third group of model constants α of formula (19) can also be obtained through the small punch test of the flat loading head: i , as shown in Table 4:

[0116] Table 4 Hardness model parameters

[0117]

[0118] S6: Substitute the material strain hardening coefficient K and strain hardening exponent n obtained in S5 into the Brinell hardness prediction model formula (19) to obtain the Brinell hardness prediction value of the material to be tested.

[0119] Furthermore, the first group of model constants and the second group of model constants are obtained by finite element analysis calibration, and the finite element analysis calculation process of the calibration model constants k1-k4 is:

[0120] When using finite element analysis software to model the small punch test, in order to obtain the model constants k1, k2, k3 and k4, E is 200GPa, σ y The load P-displacement h curve is obtained by finite element analysis. The curve data {P, h} of the finite element analysis in the range of h∈[0.15,0.3] is taken, and the P~h / d curves of the five materials are regressed to obtain the corresponding P* and m values. The k1~k4 in Table 1 can be obtained by conversion from formulas (1) and (11). The determination of k5~k8 in Table 2 is similar to the above method.

[0121] The method for obtaining the Brinell hardness of a ductile material in this embodiment is particularly suitable for testing systems of physical energy storage pressure vessels, testing systems of aerospace equipment, and testing systems of nuclear power equipment.

[0122] Example:

[0123] The method of the present invention is suitable for obtaining the Brinell hardness of ductile materials. A small punch test device with a flat loading head (punch diameter d = 4 mm, see Figure 4 ) and the small punch specimen recommended by the national standard GB / T 29459.2-2012, the disc diameter D = 10mm, the thickness B = 0.5mm, and the plane loading head is a cylinder with a diameter of 1mm. A finite element simulation model was established in the finite element analysis software, and the model constants were determined as shown in Tables 1 and 2. Finite element simulations were performed on a variety of working conditions with the same yield strength, different hardening indexes, and different hardening indexes and different yield strengths to obtain the corresponding load P-displacement h curve. The power law fitting Ph curve was used to obtain the characteristic loads P* and m. The mechanical properties parameters K and n of the material were obtained by processing according to the technical method of the present invention. Nine materials were used for experimental verification, and the loading rate was 0.1mm / min. Through analysis and comparison with the traditional Brinell hardness test of 9 materials, the Brinell hardness of the material predicted by the present invention has a maximum error of no more than 3.2%.

[0124] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for obtaining the Brinell hardness of a ductile material, characterized in that: The method for obtaining the Brinell hardness of a ductile material comprises the following steps: Step 1: Based on the equivalence between the energy density of the material under complex stress state and the energy density of the material under uniaxial stress state, a ball indentation model describing the relationship between the load P and the displacement h of the specimen under ball loading is constructed; the ball indentation model uses the power exponent m B , parameter P * , the material's strain hardening coefficient K, strain hardening exponent n and the first set of model constants k1-k4 are described; Step 2: Based on the equivalence between the energy density of the material under the complex stress state and the energy density of the material under the uniaxial stress state, a small punch test load P-displacement h model of the plane loading head is constructed to describe the relationship between the load P and the displacement h of the specimen under the loading of the small punch of the plane loading head; the small punch test load P-displacement h model of the plane loading head uses the power exponent m, the parameter P * , the strain hardening coefficient K, the strain hardening exponent n and a second set of model constants k5-k8; Step 3: According to the definition of Brinell hardness, a Brinell hardness prediction model for obtaining the Brinell hardness of the structural material to be tested is constructed in combination with the ball indentation model and the small punch test load P-displacement h model of the plane loading head; Step 4: prepare a circular thin sheet sample of the same material as the structure to be tested, perform a quasi-static test of a small punch of a plane loading head on the circular thin sheet sample, and obtain a load P-displacement h curve of the circular thin sheet sample; Step 5: Take the data of the specified section of the load P-displacement h curve of the circular thin sheet sample, perform power law fitting according to the load P-displacement h model of the small punch test of the plane loading head, and obtain the strain hardening coefficient K and strain hardening exponent n of the material; Step 6: Substitute the material strain hardening coefficient K and strain hardening exponent n obtained in step 5 into the Brinell hardness prediction model to obtain the Brinell hardness prediction value of the material to be tested.

2. The method for obtaining the Brinell hardness of a ductile material according to claim 1, characterized in that: The ball pressing model is: Where P * is the characteristic load, P is the specified load, m B is the power index, n B is a given value, K is the strain hardening coefficient, D is the diameter of the ball in the ball indentation test, and h is the depth of ball indentation.

3. The method for obtaining the Brinell hardness of a ductile material according to claim 2, characterized in that: The small punch test load P-displacement h model of the plane loading head is: Where B is the sample thickness, d is the punch diameter, and m is the power exponent.

4. The method for obtaining the Brinell hardness of a ductile material according to claim 3, characterized in that: The Brinell hardness prediction model is: The above formula HBW is the Brinell hardness, α i is the third set of model constants, and η is given by the standard.

5. The method for obtaining the Brinell hardness of a ductile material according to claim 4, characterized in that: The third set of model constants is obtained through the small punch test of the flat loading head in step 4.

6. The method for obtaining the Brinell hardness of a ductile material according to claim 1, characterized in that: The first group of model constants k1-k4 and the second group of model constants k5-k8 are calibrated and obtained respectively through finite element analysis.

7. The method for obtaining the Brinell hardness of a ductile material according to any one of claims 1 to 4, characterized in that: A test system for physical energy storage pressure vessels.

8. The method for obtaining the Brinell hardness of a ductile material according to any one of claims 1 to 4, characterized in that: Test systems for aerospace equipment.

9. The method for obtaining the Brinell hardness of a ductile material according to any one of claims 1 to 4, characterized in that: Test systems for nuclear power equipment.