Zirconium-based bentonite dephosphorization material as well as preparation method and application thereof

By modifying bentonite and modifying the metal oxide of zirconium, an efficient zirconium-based bentonite phosphorus removal material was prepared, which solved the problems of environmental risks and small adsorption capacity of lanthanum elements in the prior art, and achieved efficient phosphorus removal in water bodies. Suitable for eutrophication control of water bodies.

CN119186487AInactive Publication Date: 2024-12-27ZHEJIANG LINJIANG CHEM

Patent Information

Application Number
CN202411721151.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-28
Publication Date
2024-12-27
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lanthanum, commonly used in existing water phosphorus removal materials, has environmental risks and is small in adsorption capacity, making it difficult to effectively reduce the eutrophication of water.

Method used

Zirconium-based bentonite material is used to prepare zirconium-based bentonite phosphorus removal material with high adsorption capacity and stability by alkali modification of bentonite and to modify the metal oxide of zirconium by physical coagulation.

Benefits of technology

The zirconium-based bentonite phosphorus removal material prepared by this method has high adsorption capacity and mild reaction conditions, is environmentally friendly, can effectively reduce the phosphorus content in water, and is suitable for the removal of reservoirs and industrial wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119186487A_ABST
    Figure CN119186487A_ABST
Patent Text Reader

Abstract

The invention discloses a zirconium-based bentonite dephosphorization material as well as a preparation method and application thereof, and belongs to the field of dephosphorization materials. The invention relates to a preparation method of a zirconium-based bentonite dephosphorization material, which comprises the following steps: by taking bentonite as a matrix, carrying out alkali modification and acid modification on the bentonite to obtain a modified bentonite matrix, and modifying a zirconium metal oxide on the modified bentonite matrix by a physical coagulation method to prepare the zirconium-based bentonite dephosphorization material. The water body phosphorus removal material provided by the invention is mild in preparation condition and large in adsorption capacity, and has a good application prospect as a novel phosphorus removal agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of phosphorus removal materials, and more specifically to a zirconium-based bentonite phosphorus removal material and a preparation method and application thereof. Background Art

[0002] The problem of eutrophication of water bodies is becoming increasingly prominent. Reducing nutrients such as nitrogen and phosphorus is a practical way to prevent and control eutrophication of water bodies. Since algae are more sensitive to phosphorus, controlling the discharge of phosphorus can effectively limit the growth of algae, thereby slowing down the rate of eutrophication of water bodies. Therefore, phosphorus removal is one of the important means to reduce eutrophication of water bodies.

[0003] At present, the commonly used methods for water phosphorus removal at home and abroad mainly include biological method, chemical precipitation method and adsorption method, among which the adsorption method has the characteristics of stable effect, less environmental pollution, low cost and renewable adsorption materials. However, the materials used in the adsorption method usually contain lanthanum, which may pose environmental risks and have problems such as small adsorption capacity.

[0004] In view of the above problems, the present invention provides a zirconium-based bentonite dephosphorization material. The dephosphorization material not only has the advantages of large adsorption capacity and good stability, but also the preparation method of the dephosphorization material is environmentally friendly and has a good application prospect in water dephosphorization. Summary of the invention

[0005] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a zirconium-based bentonite phosphorus removal material and a preparation method thereof, wherein the phosphorus removal material can not only reduce the phosphorus content in water bodies, but also the preparation method has mild reaction conditions and is environmentally friendly; the second purpose of the present invention is to provide an application of a zirconium-based bentonite phosphorus removal material.

[0006] To solve the above problems, the present invention adopts the following technical solutions.

[0007] A method for preparing a zirconium-based bentonite phosphorus removal material comprises the following steps: using bentonite as a matrix, subjecting the bentonite to alkali modification and acid modification to obtain a modified bentonite matrix, and modifying zirconium metal oxide on the modified bentonite matrix by a physical coagulation method to prepare the zirconium-based bentonite phosphorus removal material.

[0008] Furthermore, the specific operations of the alkali modification and acid modification of the bentonite are as follows: (a) Alkali modification: Bentonite and sodium hydroxide powder are mixed evenly and then placed in a muffle furnace for calcination; after calcination, the mixture is naturally cooled, deionized water is added, the mixture is fully stirred, filtered, washed, and dried to obtain alkali-modified bentonite; (b) Acid modification: The alkali-modified bentonite obtained in step (a) is dispersed in a hydrochloric acid solution and shaken in a water bath; after stopping the reaction, the solution is centrifuged and washed until no chloride ions are detected, and then dried, ground, and sieved to obtain a modified bentonite matrix.

[0009] Furthermore, in the step (a), the weight ratio of bentonite to sodium hydroxide powder is 0.5-3:1.

[0010] Furthermore, in step (a), the calcination temperature of the muffle furnace is 300-600°C, and the calcination time is 1-6 h.

[0011] Furthermore, in the step (a), the suction filtration and washing are performed 2 to 6 times, and the drying is performed until the modified bentonite has a constant weight in a drying box.

[0012] Furthermore, in the step (b), the concentration of hydrochloric acid is 1-5 mol / L, the volume ratio of the mass of the alkali-modified bentonite to the hydrochloric acid is 1:2-10, the volume unit of the hydrochloric acid is mL; and the mass unit of the alkali-modified bentonite is g.

[0013] Furthermore, the water bath shaking time is 1-5 h; the drying temperature is 80-120° C.; and the pore size of the sieve used for sieving is 50-500 mesh.

[0014] Furthermore, the specific operation of preparing zirconium-based bentonite water phosphorus removal material by the physical coagulation method is as follows: dissolving a zirconium-containing compound in water to obtain a zirconium solution; immersing a modified bentonite matrix in the zirconium solution, stirring with a magnetic stirrer, aging, centrifugal washing, drying and then roasting, and naturally cooling after roasting and sieving to obtain a zirconium-based bentonite adsorption material.

[0015] Furthermore, the zirconium-containing compound is capable of generating [ZrO] after dissolving in water. 2+ The compound is one of ZrOCl2·8H2O, Zr(NO3)4 and Zr(SO4)2, and the molar concentration of the zirconium solution is 0.10~0.50 mol / L.

[0016] Furthermore, the volume ratio of the zirconium solution to the modified bentonite matrix is ​​5-50:1, the volume unit of the zirconium solution is mL; the mass unit of the modified bentonite is g.

[0017] Furthermore, the stirring time of the magnetic stirrer is 1 to 3 h, and the aging time is 8 to 36 h.

[0018] Furthermore, the number of centrifugal washing is 2 to 5 times.

[0019] Furthermore, the calcination temperature is 60-200° C., and the calcination time is 1-5 h.

[0020] Furthermore, the aperture of the sieve used for screening the zirconium-based bentonite adsorption material is 50-500 mesh.

[0021] The present invention also provides a zirconium-based bentonite phosphorus removal material, which is prepared by the above-mentioned method for preparing the zirconium-based bentonite phosphorus removal material.

[0022] The present invention also provides an application of a zirconium-based bentonite phosphorus removal material for removing phosphorus-containing substances in water bodies.

[0023] Furthermore, when used for removing phosphorus from water, the dosage concentration of the zirconium-based bentonite phosphorus removal material is preferably 0.02-2.00 g / L.

[0024] Further, the modification process of bentonite is as follows: (a) alkali modification: the bentonite and NaOH are mixed evenly, calcined in a muffle furnace at 300~600 ℃ for 1~6 h, and after natural cooling, the filtration and washing are repeated 2~6 times, and then dried in a vacuum drying oven to constant weight; (b) acid modification: the alkali-modified bentonite is immersed in 30~150 mL of hydrochloric acid with a mass concentration of 1~5 mol / L, shaken in a water bath for 1~5 h, then centrifuged and washed until no chloride ions are detected, dried and ground at 80~120 ℃, and passed through a 50~500 mesh sieve for use.

[0025] Further, the zirconium-containing compound is dissolved in water to prepare a 0.10-0.50 mol / L zirconium solution for use; the acid-base modified bentonite is immersed in the zirconium solution, stirred with a magnetic stirrer for 1-3 hours, then aged for 8-36 hours, centrifugally washed 2-5 times and then dried, and calcined at 60-200 °C for 1-5 hours; after natural cooling, it is sieved through a 50-500 mesh sieve to obtain a zirconium-based bentonite adsorption material.

[0026] Compared with the prior art, the advantages of the present invention are: The reaction conditions of this scheme are mild; moreover, the zirconium-based bentonite phosphorus removal material prepared by this method has a large adsorption capacity for phosphorus-containing substances, is environmentally friendly, and can be widely used in the removal and recovery of phosphorus-containing substances in reservoirs and industrial wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a SEM image of the modified bentonite matrix after alkali and acid modification in Example 1; Figure 2 This is the SEM image of the zirconium-based bentonite phosphorus removal material in Example 1. DETAILED DESCRIPTION

[0028] Embodiment 1:

[0029] Weigh 25 g of bentonite and 25 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine for 2.5 h. After natural cooling, add deionized water and stir thoroughly. Wash 4 times until pH = 7, filter and dry. Take 15 g of the dried bentonite and disperse it in 60 mL of 3 mol / L hydrochloric acid solution. Place it in a 30 °C water bath and shake it for 2 h. After stopping the reaction, centrifuge and wash it 5 times until no chloride ions are detected. The washed bentonite material is dried and ground at 110 °C and passed through a 200 mesh sieve to obtain the modified bentonite.

[0030] ZrOCl2·8H2O was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 100 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 °C for 3 h. After natural cooling, it was sieved through a 200 mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0031] The scanning electron microscope image (SEM image) of the modified bentonite is as follows: Figure 1 As shown; the electron microscope scanning image (SEM image) of the zirconium-based bentonite phosphorus removal material is as follows Figure 2 shown. Figure 2 The surface morphology of zirconium-based bentonite phosphorus removal materials is shown Figure 1 Compared with the surface appearance of the modified bentonite shown, there are obvious changes. Figure 2 The surface of the zirconium-based bentonite phosphorus removal material is relatively rough and has a large number of small pores; this means that the contact between the zirconium-based bentonite phosphorus removal material and the phosphate in the solution is expected to be greater, which may increase the adsorption capacity of the zirconium-based bentonite phosphorus removal material for phosphate in water.

[0032] Embodiment 2:

[0033] Weigh 25 g of bentonite and 25 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine for 2.5 h. After natural cooling, add deionized water and stir thoroughly. Wash 4 times until pH = 7, filter and dry. Take 15 g of the dried bentonite and disperse it in 60 mL of 3 mol / L hydrochloric acid solution. Place it in a 30 °C water bath and shake it for 2 h. After stopping the reaction, centrifuge and wash it 5 times until no chloride ions are detected. The washed bentonite material is dried at 110 °C and ground, and passed through a 200 mesh sieve to obtain the modified bentonite.

[0034] Zr(NO3)4 was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 100 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 °C for 3 h. After natural cooling, it was sieved through a 200-mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0035] Embodiment 3:

[0036] Weigh 25 g of bentonite and 25 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine for 2.5 h. After natural cooling, add deionized water and stir thoroughly. Wash 4 times until pH = 7, filter and dry. Take 15 g of the dried bentonite and disperse it in 60 mL of 3 mol / L hydrochloric acid solution. Place it in a water bath at 30 °C and shake it for 2 h. After stopping the reaction, centrifuge and wash it 5 times until no chloride ions are detected. Dry the washed bentonite material at 110 °C, grind it, and pass it through a 200 mesh sieve to obtain the modified bentonite.

[0037] Zr(SO4)2 was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 100 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 °C for 3 h. After natural cooling, it was sieved through a 200 mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0038] Embodiment 4:

[0039] Weigh 25 g of bentonite and 50 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine for 2.5 h. After natural cooling, add deionized water and stir thoroughly. Wash 4 times until pH = 7, filter and dry. Take 15 g of the dried bentonite and disperse it in 60 mL of 3 mol / L hydrochloric acid solution, place it in a 30 °C water bath, and shake it for 2 h. After stopping the reaction, centrifuge and wash it 5 times until no chloride ions are detected. The washed bentonite material is dried at 110 °C and ground, and passed through a 200 mesh sieve to obtain the modified bentonite.

[0040] ZrOCl2·8H2O was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 100 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 ℃ for 3 h. After natural cooling, it was sieved through a 200-mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0041] Embodiment 5:

[0042] Weigh 75 g of bentonite and 25 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine them for 2.5 h. After natural cooling, add deionized water and stir them thoroughly. Wash them 4 times until pH = 7, filter them and dry them. Take 15 g of the dried bentonite and disperse them in 105 mL of 4 mol / L hydrochloric acid solution. Place them in a 30 °C water bath and shake them for 2 h. After stopping the reaction, centrifuge and wash them 5 times until no chloride ions are detected. Dry the washed bentonite material at 110 °C, grind it, and pass it through a 200-mesh sieve to obtain the modified bentonite.

[0043] ZrOCl2·8H2O was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 100 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 ℃ for 3 h. After natural cooling, it was sieved through a 200-mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0044] Embodiment 6:

[0045] Weigh 50 g of bentonite and 25 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine for 2.5 h. After natural cooling, add deionized water and stir thoroughly. Wash 4 times until pH = 7, filter and dry. Take 15 g of the dried bentonite and disperse it in 45 mL of 5 mol / L hydrochloric acid solution. Place it in a 30 °C water bath and shake it for 2 h. After stopping the reaction, centrifuge and wash it 5 times until no chloride ions are detected. The washed bentonite material is dried at 110 °C and ground, and passed through a 200-mesh sieve to obtain the modified bentonite.

[0046] ZrOCl2·8H2O was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 100 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 ℃ for 3 h. After natural cooling, it was sieved through a 200-mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0047] Embodiment 7:

[0048] Weigh 25 g of bentonite and 25 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine for 2.5 h. After natural cooling, add deionized water and stir thoroughly. Wash 4 times until pH = 7, filter and dry. Take 15 g of the dried bentonite and disperse it in 60 mL of 3 mol / L hydrochloric acid solution. Place it in a water bath at 30 °C and shake it for 2 h. After stopping the reaction, centrifuge and wash it 5 times until no chloride ions are detected. Dry the washed bentonite material at 110 °C, grind it, and pass it through a 200 mesh sieve to obtain the modified bentonite.

[0049] ZrOCl2·8H2O was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 15 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 ℃ for 3 h. After natural cooling, it was sieved through a 200 mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0050] Embodiment 8:

[0051] Weigh 25 g of bentonite and 25 g of sodium hydroxide powder and mix them evenly. Place them in a muffle furnace at 500 °C and calcine for 2.5 h. After natural cooling, add deionized water and stir thoroughly. Wash 4 times until pH = 7, filter and dry. Take 15 g of the dried bentonite and disperse it in 60 mL of 3 mol / L hydrochloric acid solution. Place it in a water bath at 30 °C and shake it for 2 h. After stopping the reaction, centrifuge and wash it 5 times until no chloride ions are detected. Dry the washed bentonite material at 110 °C, grind it, and pass it through a 200 mesh sieve to obtain the modified bentonite.

[0052] ZrOCl2·8H2O was dissolved in water in a 100 mL volumetric flask to prepare a 0.20 mol / L zirconium solution. 3 g of the modified bentonite was immersed in 150 mL of the zirconium solution and stirred with a magnetic stirrer for 2 h. Then, it was aged for 30 h, washed by centrifugation 4 times and dried. It was then calcined at 90 ℃ for 3 h. After natural cooling, it was sieved through a 200 mesh sieve to obtain a zirconium-based bentonite phosphorus removal material.

[0053] Comparative Example 1: An appropriate amount of bentonite was placed in a muffle furnace at 500 °C and calcined for 2 h, and then cooled to room temperature to obtain calcined modified bentonite.

[0054] Test Example 1: The zirconium-based bentonite phosphorus removal materials involved in Examples 1 to 8 and the calcined modified bentonite involved in Comparative Example 1 were placed in 100 mL of a phosphorus-containing solution with an initial phosphorus concentration of 10.0 mg / L to conduct a phosphorus removal experiment; the experimental results are shown in Table 1.

[0055] Table 1 Experimental results of phosphorus removal experiment

[0056] It can be seen from Table 1 that the zirconium-based bentonite phosphorus removal material prepared by this method has a higher efficiency in terms of the adsorption capacity for phosphorus-containing substances than that of Comparative Example 1.

[0057] Test Example 2: The zirconium-based bentonite phosphorus removal material involved in Example 1 was added to 1 L of phosphorus-containing wastewater to measure the effect of different addition amounts on phosphorus removal in the water body. The experimental results are shown in Table 2.

[0058] Table 2 Experimental results of phosphorus removal effects of different dosages of zirconium-based bentonite phosphorus removal materials on water bodies

[0059] It can be seen from Table 2 that when the amount of zirconium-based bentonite phosphorus removal material added is increased to 3.0g, the phosphorus removal rate of phosphorus in phosphorus-containing wastewater does not increase significantly. Therefore, considering the cost consumption, the optimal input concentration of zirconium-based bentonite phosphorus removal material is 0.02~2.00 g / L.

Claims

1. A method for preparing a zirconium-based bentonite phosphorus removal material, characterized in that: Bentonite is used as a matrix, and the bentonite is subjected to alkali modification and acid modification to obtain a modified bentonite matrix. Zirconium metal oxide is modified on the modified bentonite matrix by a physical coagulation method to prepare a zirconium-based bentonite phosphorus removal material.

2. The method for preparing a zirconium-based bentonite phosphorus removal material according to claim 1, characterized in that: The specific operations of the alkali modification and acid modification of the bentonite are as follows: (a) Alkali modification: Bentonite and sodium hydroxide powder are mixed evenly and then placed in a muffle furnace for calcination; after calcination, the mixture is naturally cooled, deionized water is added, the mixture is fully stirred, filtered, washed, and dried to obtain alkali-modified bentonite; (b) Acid modification: The alkali-modified bentonite obtained in step (a) is dispersed in a hydrochloric acid solution and shaken in a water bath; after stopping the reaction, the solution is centrifuged and washed until no chloride ions are detected, and then dried, ground, and sieved to obtain a modified bentonite matrix.

3. The method for preparing a zirconium-based bentonite phosphorus removal material according to claim 2, characterized in that: In the step (a), the weight ratio of bentonite to sodium hydroxide powder is 0.5-3:

1.

4. The method for preparing a zirconium-based bentonite phosphorus removal material according to claim 2, characterized in that: In the step (b), the concentration of hydrochloric acid is 1-5 mol / L, and the volume ratio of the mass of the alkali-modified bentonite to the hydrochloric acid is 1:2-10.

5. The method for preparing a zirconium-based bentonite phosphorus removal material according to claim 1, characterized in that: The specific operation of preparing zirconium-based bentonite water phosphorus removal material by the physical coagulation method is as follows: dissolving a zirconium-containing compound in water to obtain a zirconium solution; immersing a modified bentonite matrix in the zirconium solution, stirring with a magnetic stirrer, aging, centrifugal washing, drying and then roasting, and naturally cooling and sieving after roasting to obtain a zirconium-based bentonite adsorption material.

6. The method for preparing a zirconium-based bentonite phosphorus removal material according to claim 5, characterized in that: The zirconium-containing compound refers to a compound that can generate [ZrO] after dissolving in water. 2+ The compound is one of ZrOCl2·8H2O, Zr(NO3)4 and Zr(SO4)2; the molar concentration of the zirconium solution is 0.10~0.50 mol / L.

7. The method for preparing a zirconium-based bentonite phosphorus removal material according to claim 5, characterized in that: The volume ratio of the zirconium solution to the modified bentonite matrix is ​​5-50:

1.

8. A zirconium-based bentonite phosphorus removal material, characterized in that: The material is prepared by the method for preparing a zirconium-based bentonite phosphorus removal material as described in any one of claims 1 to 7.

9. The use of a zirconium-based bentonite phosphorus removal material according to claim 8, characterized in that: Used to remove phosphorus-containing substances in water bodies.

10. The use of a zirconium-based bentonite phosphorus removal material according to claim 9, characterized in that: When used for water phosphorus removal, the dosage concentration of zirconium-based bentonite phosphorus removal material is 0.02~2.00 g / L.

Citation Information

Patent Citations

  • Method for preparing water dephosphorization adsorbent with bentonite

    CN106669644A

  • Method for preparing sewage high-efficiency dephosphorizing adsorbent from bentonite and application

    CN108097205A

  • Adsorbing material for phosphorus in water body and preparation and application methods thereof

    CN110280209A

  • Preparation method of La@Zr@SiO2@bentonite composite phosphorus removal adsorbent

    CN112337427A

  • Preparation and desorption method of zirconium modified zeolite-bentonite active particle dephosphorization filter material

    CN115055157A

Cited By

  • Method for processing vegetation compressed nutrient soil from bentonite

    CN120323303A

  • Synthesis method and application of X-type molecular sieve adsorbent

    CN120364717A