Easily-compacted and high-performance warm-mixing all-old material regenerated mixture and preparation method thereof

A warm-mixed all-waste recycled asphalt mixture using high-performance emulsified asphalt and a compatibilizer addresses the challenge of high-temperature issues in RAP regeneration, achieving efficient compaction and high road performance with 100% RAP utilization and reduced new asphalt use.

CN119241136APending Publication Date: 2025-01-03HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411148187.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2025-01-03

AI Technical Summary

Technical Problem

Existing asphalt pavement regeneration technologies face challenges in achieving high road performance with high reclaimed asphalt pavement (RAP) dosage due to high mixing and compacting temperatures, leading to secondary aging and poor performance, especially in cold-regenerated mixtures, which fail to utilize RAP effectively.

Method used

A warm-mixed all-waste recycled mixture comprising 100 parts of waste asphalt, 1.5 to 3.5 parts of high-performance warm-mix emulsified asphalt, and 0.2 to 0.8 parts of a compatibilizer, using a preparation method that includes heating, mixing, and curing to create a mixture that can be compacted at lower temperatures, enhancing compatibility and performance.

Benefits of technology

The solution allows for efficient compaction and high road performance at lower temperatures, avoiding secondary aging, utilizing 100% RAP, reducing new asphalt use, and improving low-temperature cracking and fatigue resistance, thus being economically and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119241136A_ABST
    Figure CN119241136A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of road engineering, in particular to an easy-to-compact and high-performance warm-mixing all-old-material regenerated mixture and a preparation method thereof.The easy-to-compact and high-performance warm-mixing all-old-material regenerated mixture is prepared from, by weight, 100 parts of waste asphalt mixture, 1.5-3.5 parts of high-performance warm-mixing emulsified asphalt and 0.2-0.8 part of compatilizer, the all-old recycled asphalt mixture disclosed by the invention is applied to the aspects of road pavement, pavement overhaul and the like, can be mixed and compacted at a relatively low temperature, and has very good construction workability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road engineering, and specifically relates to an easily compacted and high-performance warm-mixed all-waste recycled mixture and a preparation method thereof. Background Art

[0003] At present, there are two main types of asphalt pavement regeneration technologies: hot regeneration and cold regeneration. Hot-regenerated asphalt mixtures have road performance equivalent to hot-mix asphalt mixtures, but due to the high viscosity of asphalt in RAP, extremely high temperatures are required for mixing and compacting when using high RAP dosages. This leads to prominent problems such as the contradiction between RAP dosage and mixture performance, unclear economic efficiency, and secondary aging of asphalt after heating, which seriously restricts the recycling of RAP. Cold-regenerated asphalt mixtures can use more than 70% RAP, but RAP is mainly used as "black aggregate" in cold-regenerated mixtures, and the water in emulsified asphalt evaporates slowly, resulting in an excessively high void ratio in the mixture, which in turn leads to poor overall road performance of the mixture. It is generally downgraded to base structures and fails to bring out the economic value of RAP. Therefore, the development of recycled asphalt mixtures with both high road performance and high RAP dosage is a key problem to be overcome in the field of highway regeneration. Summary of the invention

[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide an easily compacted and high-performance warm-mixed all-waste recycled mixture and a preparation method thereof.

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solution: an easy-to-compact and high-performance warm-mix all-waste recycled mixture, which comprises the following raw material components by weight: 100 parts of waste asphalt mixture, 1.5 to 3.5 parts of high-performance warm-mix emulsified asphalt, and 0.2 to 0.8 parts of a compatibilizer.

[0006] In some of the embodiments, the high-performance warm mix emulsified asphalt is preferably 2 to 3 parts.

[0007] In some embodiments, the compatibilizer is preferably 0.3 to 0.6 parts.

[0008] In some of the embodiments, the waste asphalt mixture is a recycled asphalt mixture after road milling and screening, which is mainly divided into two grades: below 4.75 and above 4.75. The recycled old materials are suitable for evaluation and analysis of aggregate gradation and performance of aged asphalt. The mineral powder content in the RAP old aggregate synthetic gradation is within 4-12, and the old asphalt penetration index is preferably above 15 (0.1mm).

[0009] In some of the embodiments, the mineral powder content in the RAP old aggregate synthetic grading is preferably 6-10.

[0010] In some of the embodiments, the high-performance warm mix emulsified asphalt is an emulsion that provides excellent warm mix effect and improves the performance of the mixture, and is composed of an emulsifier, a polymer modified asphalt and a warm mix enhancer, wherein the solid content of the emulsified asphalt is more than 60%;

[0011] The emulsifier is at least one of amide, lignin and other emulsifiers;

[0012] The polymer modified asphalt is one or more polymers selected from styrene-butadiene-styrene block copolymer (SBS), styrene-butadiene rubber (SBR), waste rubber powder, etc.;

[0013] The warm mix lifting agent is selected from one or more surfactants such as dodecyl dimethyl amine oxide and alkyl alcohol amide.

[0014] In some of the embodiments, the parameters of the polymer modified asphalt are ductility (5°C) of 20-40 cm and softening point of above 60°C.

[0015] In some embodiments, the compatibilizer is a liquid mixture that improves the compatibility of emulsified asphalt with waste asphalt mixture, and the compatibilizer is at least one of aromatic oil, furfural extracted oil, naphthenic oil, epoxidized soybean oil, waste vegetable oil, and waste engine oil.

[0016] To achieve the above object, the present invention also provides the following technical solution: According to the mixed material, the preparation steps are as follows:

[0017] Step 1: Put the waste asphalt mixture into an oven for heat preservation at a temperature of 90-120°C;

[0018] Step 2: Place the insulated old material in a mixing pot or other stirring device, mix at the mixing temperature for 30-35 seconds, add the compatibilizer and mix for 90-100 seconds, and finally add the high-performance warm-mix emulsified asphalt and mix for 90 seconds; if the mineral powder content is insufficient, it is necessary to mix after adding the mineral powder, and the total mixing time is not less than 3.5 minutes. During this stage, the compatibilizer and the old asphalt mixture are fully and evenly mixed, so that the asphalt binder in the old material reaches the preset softening degree, thereby improving the fusion degree of the emulsified asphalt and the aged asphalt;

[0019] Step 3, curing the mixture obtained in step 2 at 100-110° C. for 2 hours, and then preparing the mixture into a Marshall specimen;

[0020] Step 4: Test the Marshall stability and porosity of the mixture, and determine the optimal amount of emulsified asphalt based on the requirements for porosity, stability and flow value in the specification.

[0021] Step 5. Prepare an emulsified asphalt all-recycled material mixture using steps 2 and 3 at the selected optimal emulsified asphalt dosage and test the mechanical properties and road performance of the mixture. The mechanical performance indicators include but are not limited to Marshall stability, dynamic stability, water-immersion Marshall residual stability, freeze-thaw splitting strength ratio, low-temperature bending failure strain, etc.

[0022] In some embodiments, the insulation temperature in step 1 is preferably 100-110°C.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention uses high-performance emulsified asphalt to replace hot asphalt to mix the whole old material recycled asphalt mixture. During the heating and mixing process, a large amount of water evaporates, the void ratio of the mixture is low and the strength is formed quickly. At the same time, the trace water and emulsifier remaining in the emulsified asphalt can provide a water film to improve the friction compaction performance. At the same time, the warm mix enhancer helps the asphalt particles to wet and wrap the old material, so that the emulsified asphalt whole old material recycled asphalt mixture can be mixed and compacted under the condition of 80-120°C, which is significantly lower than the mixing temperature of conventional hot mix asphalt mixture and warm mix asphalt mixture, avoiding the secondary aging problem of asphalt in the old material, having good construction and workability and low carbon and environmental protection. And based on the added compatibilizer and polymer modified asphalt, the low-temperature ductility of the aged asphalt in the old material can be restored, so that the prepared emulsified asphalt whole old material recycled asphalt mixture has excellent road performance, significantly improving the problems of low temperature and insufficient fatigue performance of conventional recycled asphalt mixture, and using all old materials, less new asphalt is added, low preparation cost, and extremely high economy and environmental protection.

[0025] Details of one or more embodiments of the present application are presented in the following drawings and descriptions to make other features, purposes and advantages of the present application more concise and easy to understand. The present application is fully described and understood through the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is the upper and lower limits of the synthetic grading of RAP material and the grading of AC13. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides a technical solution: an easily compacted and high-performance warm-mix recycled mixture of all used materials, which comprises the following raw material components by weight: 100 parts of waste asphalt mixture, 1.5 to 3.5 parts of high-performance warm-mix emulsified asphalt, and 0.2 to 0.8 parts of a compatibilizer.

[0029] The high performance warm mix emulsified asphalt is preferably 2 to 3 parts.

[0030] The compatibilizer is preferably 0.3 to 0.6 parts.

[0031] The waste asphalt mixture is a recycled asphalt mixture after road milling and screening, which is mainly divided into two grades: below 4.75 and above 4.75. The recycled old materials should be evaluated and analyzed for the aggregate gradation and the performance of aged asphalt. The mineral powder content in the RAP old aggregate synthetic gradation is within 4-12, and the old asphalt penetration index is preferably above 15 (0.1mm).

[0032] The mineral powder content in the synthetic gradation of RAP old aggregate is preferably 6-10.

[0033] The high-performance warm mix emulsified asphalt is an emulsion that provides excellent warm mix effect and improves the performance of the mixture, and is composed of an emulsifier, a polymer modified asphalt and a warm mix enhancer, wherein the solid content of the emulsified asphalt is 60%-70%;

[0034] The emulsifier is at least one of amide, lignin and other emulsifiers;

[0035] The polymer modified asphalt is one or more polymers selected from styrene-butadiene-styrene block copolymer (SBS), styrene-butadiene rubber (SBR), waste rubber powder, etc.;

[0036] The warm mix lifting agent is selected from one or more surfactants such as dodecyl dimethyl amine oxide and alkyl alcohol amide.

[0037] The parameters of the polymer modified asphalt are an ductility (5°C) of 20-40cm and a softening point of above 60°C.

[0038] The compatibilizer is a liquid mixture that improves the compatibility of emulsified asphalt with waste asphalt mixture. The compatibilizer is at least one of aromatic oil, furfural extracted oil, naphthenic oil, epoxidized soybean oil, waste vegetable oil, and waste engine oil.

[0039] A method for preparing a warm-mixed all-waste recycled material mixture that is easy to compact and has high performance. According to the mixture, the preparation steps are as follows:

[0040] Step 1: Place the waste asphalt mixture in an oven for insulation at a temperature of 90-120°C.

[0041] Step 2: Place the insulated old material in a mixing pot or other stirring device, mix at the mixing temperature for 30-35 seconds, add the compatibilizer and mix for 90-100 seconds, and finally add high-performance warm-mix emulsified asphalt and mix for 90 seconds. Select five emulsified asphalt dosages for mixing to determine the optimal emulsified asphalt dosage; if the mineral powder content is insufficient, it is necessary to mix after adding the mineral powder, and the total mixing time is not less than 3.5 minutes. During this stage, the compatibilizer and the old asphalt mixture are fully mixed and evenly mixed, so that the asphalt binder in the old material is softened to a certain extent, thereby improving the fusion degree of the emulsified asphalt and the aged asphalt;

[0042] Step 3, curing the mixture obtained in step 2 at 100-110° C. for 2 h; the purpose of this step is to simulate the transportation and paving process of actual road construction, and the mixture is prepared into test pieces according to the method in the "Test Procedure for Asphalt and Asphalt Mixtures for Highway Engineering" JTG E20-2011;

[0043] Step 4: Test the Marshall stability and porosity of the mixtures with five different emulsified asphalt dosages, and determine the optimal emulsified asphalt dosage based on the requirements for porosity, stability and flow value in the specification.

[0044] Step 5. Prepare an emulsified asphalt all-recycled material mixture using steps 2 and 3 at the selected optimal emulsified asphalt dosage and test the mechanical properties and road performance of the mixture. The mechanical performance indicators include but are not limited to Marshall stability, dynamic stability, water-immersion Marshall residual stability, freeze-thaw splitting strength ratio, low-temperature bending failure strain, etc.

[0045] The insulation temperature in step 1 is preferably 100-110°C.

[0046] Through this technical solution, it is specifically described in conjunction with the following implementation scheme:

[0047] The recycled old materials used in this embodiment come from the upper layer of a provincial highway in Liaoning Province, with gradations of AC-13 and aggregate material of basalt. For the milled RAP old materials, the aggregate gradation and the performance of the aged asphalt are evaluated and analyzed to determine the degree of aging. The compatibilizer used is a yellow low-viscosity liquid, and the specific indicators are shown in Table 1. The high-performance warm-mix emulsified asphalt is a slow-cracking cationic emulsified asphalt, and the specific indicators are shown in Table 2.

[0048] Table 1 Basic information of compatibilizer

[0049] Technical indicators result 60℃ viscosity, cp 56 Flash point, °C 226 Saturated content, % 11 Aroma content, % 28

[0050] Table 2 Basic indicators of emulsified asphalt

[0051] Test Project Test results 1.18mm sieve residue (%) 0 1 day 0.02 5 days 0.6 Solid content (%) 65 Needle penetration (25℃, 0.1mm) 60 Softening point (R&B, ℃) 68 Ductility (5℃, mm) 30

[0052] According to the T0722-1993 centrifugal separation method in "JTG E20-2011 Highway Engineering Asphalt and Asphalt Mixture Test Procedure", the old asphalt was extracted and the aggregate gradation was analyzed. The final synthetic gradation is shown in Figure 1 The extraction solution was used to obtain aged asphalt using the rotary evaporation method of T0727-2011. The basic indicators of the aged asphalt were tested to determine the degree of aging. The test results are shown in Table 3.

[0053] Table 3 Performance indexes of recycled asphalt

[0054] Technical indicators Needle penetration / (0.1mm) Softening point / ℃ 10℃ elongation / mm result 16 70 5

[0055] Depend on Figure 1 It can be seen that the synthetic grading of RAP material below 0.075 is slightly higher than the grading range, and the others are between the upper and lower limits of AC-13 grading.

[0056] The preparation of emulsified asphalt warm mix all-waste recycled mixture includes the following steps:

[0057] S1. Keep the old material in an oven at 110℃ for 3h.

[0058] S2. Place the old material in a mixing pot, mix at 100℃ for 30s, add the compatibilizer and mix for 90s, and finally add high-performance warm-mix emulsified asphalt and mix for 90s. The total mixing time is 3.5min. The amount of compatibilizer is 0.3% of the total amount of old material. Five emulsified asphalt dosages are selected, and the emulsified asphalt dosages are 1.5%, 2%, 2.5%, 3%, and 3.5% of the old material mass, respectively, to prepare emulsified asphalt warm-mixed all-old material recycled mixtures.

[0059] S3. The mixture obtained in S2 is cured at a compaction temperature of 100°C for 2 hours to simulate the transportation and paving process in an actual project.

[0060] S4. The volume and mechanical indices of the test species mixture, the Marshall stability, flow value and void ratio under different emulsified asphalt dosages are shown in Table 4.

[0061] Table 4 Marshall stability, flow value and void ratio results at different emulsified asphalt dosages

[0062] Emulsified asphalt dosage Void ratio Marshall stability Stream Value 1.5 6.4 14.845 2.896 2 5.13 15.05 3.132 2.5 3.51 16.385 3.29 3 3.23 14.28 3.8 3.5 2.5 13.645 5.82 Technical requirements 3-5 ≥8 2-4

[0063] It can be seen from Table 4 that with the increase in the amount of emulsified asphalt, the void ratio of the emulsified asphalt warm mix fully recycled mixture gradually decreases, the Marshall stability first increases and then decreases, and the flow value gradually increases. When the amount of emulsified asphalt is 2.5%, the three indicators of the warm mix fully recycled mixture are the best. Therefore, the optimal amount of emulsified asphalt is determined to be 2.5%.

[0064] S5. Prepare a warm-mixed recycled mixture of all old materials by using step 2 under the selected optimal emulsified asphalt dosage, and test the road performance of the mixture. In this embodiment, the mixture is prepared into corresponding test pieces according to the method in "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" JTG E20-2011, and the dynamic stability (T0719-2011), water immersion residual stability (T 0709-2011), freeze-thaw splitting tensile strength ratio TSR (T 0729-2000), and low-temperature bending failure strain (T 0715-2011) of the test material are tested. The test results are shown in Table 5. The results show that the road performance of the invented warm-mixed recycled mixture of all old materials meets the requirements of the specification, has good road performance, and uses all old materials, which is very economical and environmentally friendly.

[0065] Table 5 Road performance of warm mix recycled material

[0066] Technical indicators Dynamic stability times / mm Residual stability after immersion in water / % Freeze-thaw splitting strength ratio TSR / % Low temperature bending failure strain Technical requirements ≥1000 ≥80 ≥75 ≥2000 Test Results 3000 93.83 85.6 2546

[0067] In summary, the present invention uses high-performance warm-mix emulsified asphalt to replace hot asphalt to mix the all-old recycled asphalt mixture, and significantly improves the mixing and compacting characteristics of the mixture through the emulsifier water film and the warm-mix enhancer, and reduces the mixing temperature to 50-70°C; and based on the added compatibilizer and polymer-modified asphalt, the low-temperature ductility of the aged asphalt in the old material can be restored, so that the prepared warm-mix all-old recycled asphalt mixture has excellent road performance, and uses only old materials, less new asphalt is added, the preparation cost is low, and it has extremely high economy and environmental protection.

[0068] The all-old recycled asphalt mixture of the present invention is used in road paving, road overhaul and other aspects. It can be mixed and compacted at a relatively low temperature, has good construction and workability, avoids problems such as secondary aging of asphalt caused by high temperature, realizes 100% utilization of old materials, saves resources, and effectively improves the low-temperature cracking and fatigue performance of the recycled mixture, so that the all-old recycled asphalt mixture has excellent comprehensive performance and is an environmentally friendly asphalt pavement material.

[0069] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A warm-mixed recycled material mixture that is easy to compact and has high performance, characterized by: Calculated by weight, the raw material components include: 100 parts of waste asphalt mixture, 1.5 to 3.5 parts of high-performance warm-mix emulsified asphalt, and 0.2 to 0.8 parts of compatibilizer.

2. The easy-to-compact and high-performance warm-mix recycled material mixture according to claim 1, characterized in that: The high performance warm mix emulsified asphalt is preferably 2 to 3 parts.

3. The easy-to-compact and high-performance warm-mix all-waste recycled material mixture according to claim 1, characterized in that: The compatibilizer is preferably 0.3 to 0.6 parts.

4. The easy-to-compact and high-performance warm-mix recycled material mixture according to claim 1, characterized in that: The waste asphalt mixture is a recycled asphalt mixture after road milling and screening, which is mainly divided into two grades: below 4.75 and above 4.

75. The recycled old materials should be evaluated and analyzed for the aggregate gradation and the performance of aged asphalt. The mineral powder content in the RAP old aggregate synthetic gradation is within 4-12, and the old asphalt penetration index is preferably above 15 (0.1mm).

5. The easy-to-compact and high-performance warm-mix recycled material mixture according to claim 1, characterized in that: The mineral powder content in the synthetic gradation of RAP old aggregate is preferably 6-10.

6. The easy-to-compact and high-performance warm-mix recycled material mixture according to claim 1, characterized in that: The high-performance warm mix emulsified asphalt is an emulsion that provides excellent warm mix effect and improves the performance of the mixture, and is composed of an emulsifier, a polymer modified asphalt and a warm mix enhancer, wherein the solid content of the emulsified asphalt is more than 60%; The emulsifier is at least one of amide, lignin and other emulsifiers; The polymer modified asphalt is one or more polymers selected from styrene-butadiene-styrene block copolymer (SBS), styrene-butadiene rubber (SBR), waste rubber powder, etc.; The warm mix lifting agent is selected from one or more surfactants such as dodecyl dimethyl amine oxide and alkyl alcohol amide.

7. The easy-to-compact and high-performance warm-mix recycled material mixture according to claim 6, characterized in that: The parameters of the polymer modified asphalt are an ductility (5°C) of 20-40cm and a softening point of above 60°C.

8. The easy-to-compact and high-performance warm-mix recycled material mixture according to claim 1, characterized in that: The compatibilizer is a liquid mixture for improving the compatibility of emulsified asphalt and waste asphalt mixture, and the compatibilizer is at least one of aromatic oil, furfural extracted oil, cycloparaffin oil, epoxidized soybean oil, waste vegetable oil and waste engine oil.

9. A method for preparing a warm-mixed recycled material mixture that is easy to compact and has high performance, characterized in that: The mixed material according to any one of claims 1 to 8, wherein the preparation steps are: Step 1: Place the waste asphalt mixture in an oven for insulation at a temperature of 90-120°C. Step 2: Place the insulated old material in a mixing pot or other stirring device, mix at the mixing temperature for 30-35 seconds, add the compatibilizer and mix for 90-100 seconds, and finally add the high-performance warm-mix emulsified asphalt and mix for 90 seconds; if the mineral powder content is insufficient, it is necessary to mix after adding the mineral powder, and the total mixing time is not less than 3.5 minutes. During this stage, the compatibilizer and the old asphalt mixture are fully and evenly mixed, so that the asphalt binder in the old material reaches the preset softening degree, thereby improving the fusion degree of the emulsified asphalt and the aged asphalt; Step 3, curing the mixture obtained in step 2 at 100-110° C. for 2 hours, and then preparing the mixture into a Marshall specimen; Step 4: Test the Marshall stability and porosity of the mixture, and determine the optimal amount of emulsified asphalt based on the requirements for porosity, stability and flow value in the specification. Step 5. Prepare an emulsified asphalt all-recycled material mixture using steps 2 and 3 at the selected optimal emulsified asphalt dosage and test the mechanical properties and road performance of the mixture. The mechanical performance indicators include but are not limited to Marshall stability, dynamic stability, water-immersion Marshall residual stability, freeze-thaw splitting strength ratio, low-temperature bending failure strain, etc.

10. The method for preparing a high-performance warm-mixed recycled material mixture that is easy to compact according to claim 9, characterized in that: The insulation temperature in step 1 is preferably 100-110°C.