Foaming polyurethane thermal insulation material containing neutral water and preparation method thereof
The use of neutral water and specific polyoxypropylene triols and hydroxyindole ketones in foamed polyurethane insulation materials addresses environmental concerns and strengthens compression resistance, ensuring effective thermal insulation and structural integrity.
Patent Information
- Application Number
- CN202411417750.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2025-01-03
AI Technical Summary
Traditional foamed polyurethane thermal insulation materials use harmful chemical foaming agents and have insufficient compression strength, leading to environmental pollution and deformation in high-load or vibration environments.
A foamed polyurethane thermal insulation material using neutral water as a foaming agent and incorporating terminal primary hydroxyl polyoxypropylene triols with different hydroxyl values and hydroxyindole ketones to enhance cross-linking density and compressive strength, along with fillers like diatomaceous earth and calcium carbonate.
The material achieves improved thermal insulation performance, reduced environmental impact, and enhanced compression strength, preventing deformation and damage under external pressures.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation materials, and in particular to a foamed polyurethane thermal insulation material containing neutral water and a preparation method thereof. Background Art
[0002] As the world pays more and more attention to energy conservation and environmental protection, the demand for high-efficiency thermal insulation materials in the construction and industrial fields continues to grow. Traditional foamed polyurethane thermal insulation materials have excellent thermal insulation performance, but they often use chemical foaming agents such as Freon. These chemical foaming agents are not only harmful to the environment, but may also release harmful substances during production and use, which does not meet the requirements of modern green development.
[0003] In recent years, people have been committed to finding more environmentally friendly and sustainable insulation material solutions. Neutral water, as a non-toxic, harmless, widely available and chemically stable substance, has gradually attracted the attention of researchers. Introducing neutral water into the preparation process of foamed polyurethane insulation materials is expected to reduce the negative impact on the environment without reducing the insulation performance, thus achieving green production of insulation materials.
[0004] At the same time, with the continuous advancement of science and technology, the research and development of new materials in the field of materials science is also accelerating. In some special environments, such as long-term high-load pressure or frequent mechanical vibration, the existing insulation materials have insufficient compression strength and are prone to deformation or even local damage, affecting the insulation effect and service life. In order to ensure that the insulation materials can maintain their shape and structural integrity during installation and use, and will not be easily deformed or damaged even under certain external pressures, such as the weight of the building itself, personnel activities or equipment placement, the development of a neutral water-foamed polyurethane insulation material with high compression strength is an urgent problem to be solved. Summary of the invention
[0005] The invention provides a foamed polyurethane thermal insulation material containing neutral water and a preparation method thereof, which solves the problem of low compression strength of the thermal insulation material in the related art.
[0006] The technical scheme of the present invention is as follows: The present invention provides a foamed polyurethane thermal insulation material containing neutral water, comprising the following component raw materials in parts by weight: 30-40 parts of polyphenyl polymethylene polyisocyanate, 20-30 parts of terminal primary hydroxyl polyoxypropylene triol, 0.5-1.5 parts of catalyst, 1-3 parts of neutral water, 1-1.5 parts of foam stabilizer, and 3-5 parts of filler; The terminal primary hydroxyl polyoxypropylene triol comprises a first terminal primary hydroxyl polyoxypropylene triol and a second terminal primary hydroxyl polyoxypropylene triol, and the first terminal primary hydroxyl polyoxypropylene triol and the second terminal primary hydroxyl polyoxypropylene triol have different hydroxyl values.
[0007] As a further technical solution, the hydroxyl value of the first primary hydroxyl polyoxypropylene triol is 32-36 mgKOH / g, the hydroxyl value of the second primary hydroxyl polyoxypropylene triol is 53-59 mgKOH / g, and the mass ratio of the first primary hydroxyl polyoxypropylene triol to the second primary hydroxyl polyoxypropylene triol is 2:1-3.
[0008] As a further technical solution, the raw material further comprises a hydroxyindole ketone compound, and the mass ratio of the hydroxyindole ketone compound to the polyphenyl polymethylene polyisocyanate is 1-2:20.
[0009] In the present invention, the addition of hydroxyindole ketone compounds not only participates in the formation of the polyurethane network, increases the cross-linking density of the material, makes the molecular structure more compact, and thus improves the compressive strength, but also can form a relatively hydrophobic area on the surface or inside of the material, reduces the channels for water molecule penetration, thereby hindering the entry of water molecules and reducing the water absorption rate of the thermal insulation material.
[0010] As a further technical solution, the hydroxyindole ketone compound includes one or more of 1-(hydroxymethyl)-indole-3-dione, 7-hydroxy-2-indole ketone, and 4-hydroxyindole ketone.
[0011] As a further technical solution, the catalyst includes one or more of dimethylcyclohexylamine, triethylenediamine, and triethylamine.
[0012] As a further technical solution, the foam stabilizer is silicone oil.
[0013] As a further technical solution, the filler includes one or more of diatomaceous earth, calcium carbonate, and talc.
[0014] In the present invention, neutral water is added as a foaming agent. Compared with traditional chemical foaming agents, neutral water is a non-toxic and harmless substance that does not release gases or chemicals that are harmful to the environment. Using neutral water as a foaming agent can greatly reduce environmental pollution in the production process of thermal insulation materials, which meets the needs of modern society for environmentally friendly materials. In addition, neutral water can form uniform and fine bubbles during the foaming process, which can effectively prevent the transfer of heat and improve the thermal insulation performance and compression strength of the thermal insulation material.
[0015] The present invention also provides a method for preparing a foamed polyurethane thermal insulation material containing neutral water, comprising the following steps: S1, mixing terminal primary hydroxyl polyoxypropylene triol, catalyst, neutral water, foam stabilizer and filler to obtain a mixed solution; S2, adding polyphenyl polymethylene polyisocyanate into the mixed solution, stirring evenly and then curing and forming, so as to obtain a foamed polyurethane thermal insulation material.
[0016] As a further technical solution, the mixing time is 10 to 15 minutes.
[0017] As a further technical solution, the stirring time is 20 to 30 seconds.
[0018] The working principle and beneficial effects of the present invention are: In the present invention, terminal primary hydroxyl polyoxypropylene triols with different hydroxyl values are added as raw materials to exert the synergistic effect of the two, optimize the cross-linking structure, and enable the foamed polyurethane thermal insulation material to better disperse the compressive stress, avoid damage caused by local stress concentration, and thus improve the compressive strength. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] In the following examples and comparative examples: First-terminal primary hydroxyl polyoxypropylene triol: hydroxyl value is 32~36mgKOH / g, glycerol initiator, viscosity is 400~600cps, manufacturer is Jiangsu Senfeida Chemical Co., Ltd.; Second-terminal primary hydroxyl polyoxypropylene triol: hydroxyl value is 53~59mgKOH / g, glycerol initiator, viscosity is 750~950cps, manufacturer is Jiangsu Senfeida Chemical Co., Ltd.; Polyether polyol: Model is EP-330N.
[0021] Example 1 S1, mixing 20 parts of terminal primary hydroxyl polyoxypropylene triol, 0.5 parts of dimethylcyclohexylamine, 1 part of neutral water, 1 part of silicone oil, and 3 parts of diatomaceous earth for 10 minutes, and mixing evenly to obtain a mixed solution, wherein the terminal primary hydroxyl polyoxypropylene triol is the first terminal primary hydroxyl polyoxypropylene triol; S2. Add 30 parts of polyphenyl polymethylene polyisocyanate into the mixed solution, stir for 20 seconds, and solidify and shape after stirring evenly to obtain a foamed polyurethane thermal insulation material.
[0022] Example 2 S1, mixing 25 parts of terminal primary hydroxyl polyoxypropylene triol, 1 part of triethylene diamine, 2 parts of neutral water, 1.2 parts of silicone oil, and 4 parts of calcium carbonate for 12 minutes, and mixing evenly to obtain a mixed solution, wherein the terminal primary hydroxyl polyoxypropylene triol is the first terminal primary hydroxyl polyoxypropylene triol; S2. Add 35 parts of polyphenyl polymethylene polyisocyanate into the mixed solution, stir for 25 seconds, and solidify and shape after stirring evenly to obtain a foamed polyurethane thermal insulation material.
[0023] Example 3 S1, mixing 30 parts of terminal primary hydroxyl polyoxypropylene triol, 1.5 parts of triethylamine, 3 parts of neutral water, 1.5 parts of silicone oil, and 4 parts of talcum powder for 15 minutes, and mixing evenly to obtain a mixed solution, wherein the terminal primary hydroxyl polyoxypropylene triol is the first terminal primary hydroxyl polyoxypropylene triol; S2. Add 40 parts of polyphenyl polymethylene polyisocyanate into the mixed solution, stir for 30 seconds, and solidify and shape after stirring evenly to obtain a foamed polyurethane thermal insulation material.
[0024] Example 4 Compared with Example 3, Example 4 is different in that the terminal primary hydroxyl polyoxypropylene triol is the second terminal primary hydroxyl polyoxypropylene triol.
[0025] Example 5 Compared with Example 3, the difference of Example 5 is that the 30 parts of terminal primary hydroxyl polyoxypropylene triol include 22 parts of first terminal primary hydroxyl polyoxypropylene triol and 8 parts of second terminal primary hydroxyl polyoxypropylene triol.
[0026] Example 6 Compared with Example 3, the difference of Example 6 is that the 30 parts of terminal primary hydroxyl polyoxypropylene triol include 20 parts of first terminal primary hydroxyl polyoxypropylene triol and 10 parts of second terminal primary hydroxyl polyoxypropylene triol.
[0027] Example 7 Compared with Example 3, the difference of Example 7 is that 30 parts of terminal primary hydroxyl polyoxypropylene triol include 12 parts of first terminal primary hydroxyl polyoxypropylene triol and 18 parts of second terminal primary hydroxyl polyoxypropylene triol.
[0028] Example 8 Compared with Example 3, the difference of Example 8 is that the 30 parts of terminal primary hydroxyl polyoxypropylene triol include 10 parts of first terminal primary hydroxyl polyoxypropylene triol and 20 parts of second terminal primary hydroxyl polyoxypropylene triol.
[0029] Example 9 S1, mixing 30 parts of terminal primary hydroxyl polyoxypropylene triol, 1.5 parts of triethylamine, 3 parts of neutral water, 1.5 parts of silicone oil, 4 parts of talcum powder, and 1 part of 7-hydroxy-2-indolone for 15 minutes, and mixing evenly to obtain a mixed solution, wherein the 30 parts of terminal primary hydroxyl polyoxypropylene triol include 10 parts of first terminal primary hydroxyl polyoxypropylene triol and 20 parts of second terminal primary hydroxyl polyoxypropylene triol; S2. Add 40 parts of polyphenyl polymethylene polyisocyanate into the mixed solution, stir for 30 seconds, and solidify and shape after stirring evenly to obtain a foamed polyurethane thermal insulation material.
[0030] Example 10 Compared with Example 9, the difference in Example 10 is that the added amount of 7-hydroxy-2-indolone is 2 parts.
[0031] Embodiment 11 Compared with Example 9, the difference in Example 11 is that the added amount of 7-hydroxy-2-indolone is 4 parts.
[0032] Example 12 Compared with Example 9, the difference in Example 12 is that the added amount of 7-hydroxy-2-indolone is 6 parts.
[0033] Comparative Example 1 Compared with Example 3, the difference in Comparative Example 1 is that the terminal primary hydroxyl polyoxypropylene triol is replaced by an equal amount of polyether polyol.
[0034] The foamed polyurethane thermal insulation materials prepared in Examples 1 to 8 and Comparative Example 1 were tested according to the following method: 1. Compression strength: According to the test method specified in GB / T 8813-2020 "Determination of compression properties of rigid foam plastics", the compression strength of the sample is tested. The sample size is 50mm×50mm×50mm, and the compression speed is 5mm / min.
[0035] The test results are shown in Table 1 below: Table 1 Compressive strength test results of the foamed polyurethane thermal insulation materials prepared in Examples 1 to 8 and Comparative Example 1
[0036] Compared with Comparative Example 1, Example 3 replaces the polyether polyol with terminal primary hydroxyl polyoxypropylene triol. As a result, the compressive strength of Example 3 is higher than that of Comparative Example 1, indicating that the addition of terminal primary hydroxyl polyoxypropylene triol can improve the compressive strength of the foamed polyurethane thermal insulation material. Compared with Examples 3 and 4, Examples 5 to 8 simultaneously add the first terminal primary hydroxyl polyoxypropylene triol and the second terminal primary hydroxyl polyoxypropylene triol. As a result, the compressive strength of Examples 5 to 8 is higher than that of Examples 3 and 4, indicating that the first terminal primary hydroxyl polyoxypropylene triol and the second terminal primary hydroxyl polyoxypropylene triol play a synergistic role and can improve the compressive strength of the foamed polyurethane thermal insulation material. In Examples 5 to 8, different mass ratios of the first terminal primary hydroxyl polyoxypropylene triol and the second terminal primary hydroxyl polyoxypropylene triol are added. As a result, the compressive strength of Examples 6 and 7 is higher than that of Examples 5 and 8, indicating that when the mass ratio of the first terminal primary hydroxyl polyoxypropylene triol and the second terminal primary hydroxyl polyoxypropylene triol is 2:1~3, the obtained foamed polyurethane thermal insulation material has a higher compressive strength.
[0037] The foamed polyurethane thermal insulation materials prepared in Examples 7 and 9 to 12 were tested according to the following method: Water absorption rate: According to the test method specified in GB / T 8810-2005 "Determination of water absorption rate of rigid foam plastics", the water absorption rate of the sample is tested. The test results are shown in Table 2 below: Table 2 Water absorption performance test results of the foamed polyurethane thermal insulation materials prepared in Examples 7 and 9 to 12
[0038] Compared with Example 7, Examples 9 to 12 add hydroxyindole ketone compounds, and the water absorption of Examples 9 to 12 is less than that of Example 7, indicating that the addition of hydroxyindole ketone compounds can reduce the water absorption of foamed polyurethane thermal insulation materials. In Examples 9 to 12, different masses of hydroxyindole ketone compounds are added, and the water absorption of Examples 10 and 11 is less than that of Examples 9 and 12, indicating that when the mass ratio of hydroxyindole ketone compounds to polyphenyl polymethylene polyisocyanate is 1 to 2:20, the water absorption of the obtained foamed polyurethane thermal insulation material is smaller.
[0039] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A foamed polyurethane thermal insulation material containing neutral water, characterized in that: The invention comprises the following raw materials in parts by weight: 30-40 parts of polyphenyl polymethylene polyisocyanate, 20-30 parts of terminal primary hydroxyl polyoxypropylene triol, 0.5-1.5 parts of catalyst, 1-3 parts of neutral water, 1-1.5 parts of foam stabilizer and 3-5 parts of filler; the terminal primary hydroxyl polyoxypropylene triol comprises a first terminal primary hydroxyl polyoxypropylene triol and a second terminal primary hydroxyl polyoxypropylene triol, and the first terminal primary hydroxyl polyoxypropylene triol and the second terminal primary hydroxyl polyoxypropylene triol have different hydroxyl values.
2. The foamed polyurethane thermal insulation material containing neutral water according to claim 1, characterized in that: The hydroxyl value of the first terminal primary hydroxyl polyoxypropylene triol is 32-36 mgKOH / g, the hydroxyl value of the second terminal primary hydroxyl polyoxypropylene triol is 53-59 mgKOH / g, and the mass ratio of the first terminal primary hydroxyl polyoxypropylene triol to the second terminal primary hydroxyl polyoxypropylene triol is 2:1-3.
3. The foamed polyurethane thermal insulation material containing neutral water according to claim 1, characterized in that: The raw materials also include hydroxyindole ketone compounds, and the mass ratio of the hydroxyindole ketone compounds to the polyphenyl polymethylene polyisocyanate is 1-2:
20.
4. The foamed polyurethane thermal insulation material containing neutral water according to claim 3, characterized in that: The hydroxyindole ketone compound includes one or more of 1-(hydroxymethyl)-indole-3-dione, 7-hydroxy-2-indole ketone and 4-hydroxyindole ketone.
5. The foamed polyurethane thermal insulation material containing neutral water according to claim 1, characterized in that: The catalyst includes one or more of dimethylcyclohexylamine, triethylenediamine, and triethylamine.
6. The foamed polyurethane thermal insulation material containing neutral water according to claim 1, characterized in that: The foam stabilizer is silicone oil.
7. The foamed polyurethane thermal insulation material containing neutral water according to claim 1, characterized in that: The filler includes one or more of diatomaceous earth, calcium carbonate and talc.
8. The method for preparing a foamed polyurethane thermal insulation material containing neutral water according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, mixing terminal primary hydroxyl polyoxypropylene triol, catalyst, neutral water, foam stabilizer and filler to obtain a mixed solution; S2, adding polyphenyl polymethylene polyisocyanate into the mixed solution, stirring evenly and then curing and forming, so as to obtain a foamed polyurethane thermal insulation material.
9. The method for preparing a foamed polyurethane thermal insulation material containing neutral water according to claim 8, characterized in that: The mixing time is 10 to 15 minutes.
10. The method for preparing a foamed polyurethane thermal insulation material containing neutral water according to claim 8, characterized in that: The stirring time is 20 to 30 seconds.