Packaging material for molding, packaging case, and power storage device

By using a metal foil layer, a heat-resistant resin layer, a hot-weld resin layer and an outer adhesive layer containing an insulating enhancer in the lithium-ion battery packaging material, the pinhole of the lithium-ion battery packaging material is solved in the molding processing. and the problem of mechanical strength achieves high penetration strength and insulation, improving the safety and performance of the battery.

CN221794044UActive Publication Date: 2024-10-01LISSENOK PACKAGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202322847923.8
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Priority Date
2023-09-07
Filing Date
2023-10-23
Publication Date
2024-10-01
Estimated Expiration
2033-10-23

AI Technical Summary

Technical Problem

The existing lithium-ion battery packaging materials are prone to pinholes during molding and processing, making it difficult to achieve large capacity and high mechanical strength of the battery, and are prone to damage due to external forces.

Method used

A packaging material consisting of a metal foil layer, a heat-resistant resin layer, a hot-weld resin layer, an outer adhesive layer and an inner adhesive layer are used. The outer adhesive layer contains an insulating enhancer and an insulating enhancer. The number average particle size is 0.01 μm to 3 μm, the specific surface area is 1 m2/g or more, the volume resistivity is 1×1012Ωcm or more, and an outer adhesive layer is provided between the metal foil layer and the heat-resistant resin layer to ensure high poking Strength and insulation.

Benefits of technology

It improves the penetration strength and insulation of the packaging material, enhances the durability of external force impact, and ensures the safety and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221794044U_ABST
    Figure CN221794044U_ABST
Patent Text Reader

Abstract

The utility model relates to a packaging material for forming processing, a packaging shell and an electrical storage device. A packaging material (1) for molding is provided with a metal foil layer (2), a heat-resistant resin layer (3) disposed on the outer surface side of the metal foil layer (2), and a heat-fusible resin layer (4) disposed on the inner surface side of the metal foil layer (2), and an outer adhesive layer (5R) is provided between the metal foil layer (2) and the heat-resistant resin layer (3). An inner adhesive layer (6) is provided between the metal foil layer (2) and the heat-fusible resin layer (4). The outer adhesive layer (5R) contains an insulation reinforcing agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a packaging material for molding, a packaging shell and an electric storage device. It should be noted that the packaging material can be used as a packaging material for non-fixed (laptop computers, mobile phones, car-mounted, etc.) and fixed electric storage devices (lithium ion batteries, etc.), and can also be used as a packaging material for food and medicine.

[0002] In addition, in the present specification and claims, unless otherwise clearly indicated herein, various physical property values ​​(specific surface area, volume resistivity, tensile strength at break, tensile elongation at break, etc.) are values ​​at room temperature. Background Art

[0003] Among various power storage devices, for example, lithium-ion batteries used in mobile devices (e.g., smartphones, tablet computers, and laptop computers), the battery body is packaged with a packaging material. As the packaging material, for example, a packaging material formed of a metal-resin laminated material in which a resin film is laminated on the inner surface and the outer surface of a metal foil is used. For the packaging material, in order to form a space for accommodating the battery body, a predetermined forming process such as a drawing process (e.g., a deep drawing process, a stretching process) can be performed.

[0004] Such batteries are generally required to be thinner and lighter. If the metal foil and resin films are thinned in the packaging material to meet this requirement, the probability of pinholes being generated during the molding of the packaging material becomes higher. On the other hand, if the molding depth is shallower to suppress the generation of pinholes, it becomes difficult to cope with the increase in battery capacity. In addition, if the resin film is thinned, the puncture strength of the packaging material is reduced, and the battery is easily broken due to external impact.

[0005] The packaging materials used for non-stationary (mobile, portable, etc.) power storage devices, such as the lithium-ion batteries for mobile devices, are more likely to be damaged by external forces such as impact, vibration, and external pressure than those used for stationary power storage devices. Therefore, packaging materials formed of metal-resin laminates are also required to have mechanical strength that can withstand external forces, especially excellent puncture resistance.

[0006] In order to improve the puncture strength of packaging materials, Patent Document 1 discloses the use of biaxially stretched polyester or biaxially stretched polyamide films as the outer layer of packaging materials. In addition, Patent Document 2 discloses the use of a heat-fusible resin film formed by laminating and integrating covering layers containing random copolymer polypropylene on the inner and outer surfaces of an intermediate layer containing block copolymer polypropylene as the inner layer of packaging materials. In addition, as a document that discloses improving the puncture strength of packaging materials, there is, for example, Patent Document 3.

[0007] It should be noted that, although the purpose is not to improve the puncture strength of the packaging material, as documents that disclose the technology for coloring the outer surface of the packaging material, there are Patent Documents 4 and 5. These documents disclose that carbon black, titanium oxide, etc. are added as coloring pigments for coloring the outer surface of the packaging material to the adhesive layer provided on the outer surface side of the metal foil layer of the packaging material.

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2022-50325 (paragraph

[0022] , etc.)

[0010] Patent Document 2: Japanese Patent Application Publication No. 2015-143107 (paragraph

[0028] , etc.)

[0011] Patent Document 3: Japanese Patent Application Publication No. 2020-161326

[0012] Patent Document 4: Japanese Patent Application Publication No. 2017-10941

[0013] Patent Document 5: International Publication No. 2019 / 070078 Utility Model Content

[0014] Issues to be Solved by Utility Models

[0015] In recent years, as the capacity of power storage devices such as lithium-ion batteries has increased, the safety of power storage devices has become increasingly important. As a result, packaging materials are being required to have higher puncture strength and higher insulation properties.

[0016] The present invention is made in view of the above technical background, and an object of the present invention is to provide a packaging material and a packaging case for molding having high puncture strength and high insulation, and a power storage device using the packaging material.

[0017] Means for solving problems

[0018] The utility model provides the following means.

[0019] 1) A packaging material for molding, comprising a metal foil layer, a heat-resistant resin layer disposed on the outer surface side of the metal foil layer, and a heat-fusible resin layer disposed on the inner surface side of the metal foil layer, an outer adhesive layer being disposed between the metal foil layer and the heat-resistant resin layer, and an inner adhesive layer being disposed between the metal foil layer and the heat-fusible resin layer,

[0020] The outer adhesive layer contains an insulation reinforcing agent.

[0021] 2) The molding packaging material according to the above Item 1, wherein the insulation reinforcing agent is an insulation reinforcing particle, and

[0022] The number average particle size of the insulation-enhancing particles is in the range of 0.01 μm to 3 μm.

[0023] 3) The molding packaging material according to the above item 1 or 2, wherein the insulation reinforcing agent is an insulation reinforcing particle, and

[0024] The specific surface area of ​​the aforementioned insulating enhanced particles is 1m 2 / g or above.

[0025] 4) The molding packaging material according to any one of the above 1 to 3, wherein the insulation reinforcing agent is an insulation reinforcing particle, and

[0026] The volume resistivity of the insulating reinforcing particles is 1×10 12 Ωcm or more.

[0027] 5) The molding packaging material according to any one of the above items 1 to 4, wherein the outer adhesive layer is formed of a cured film of an outer adhesive composition containing an outer adhesive and the insulation reinforcing agent,

[0028] The tensile elongation at break of the cured film of the outer adhesive composition is defined as L.

[0029] When the tensile elongation at break of a cured film of an external adhesive composition containing the external adhesive but not containing the insulation reinforcing agent is defined as L0,

[0030] The aforementioned L satisfies the following relational expression 1.

[0031] 15%≤{(L-L0) / L0}×100%≤250%…(Formula 1).

[0032] 6) The molding packaging material as described in any one of the above 1 to 5, wherein the outer adhesive layer has a thickness of 2 g / m 2 ~10g / m 2 The coating amount in the range of is provided between the metal foil layer and the heat-resistant resin layer,

[0033] The content of the insulating reinforcing agent in the outer adhesive layer is 0.2 g / m 2 ~1.0g / m 2 within the range.

[0034] 7) A packaging case, which is formed by deep drawing or stretching the packaging material for molding as described in any one of 1 to 6 above.

[0035] 8) A power storage device comprising a power storage device body and a packaging case packaging the power storage device body,

[0036] As the package case, there is provided the package case described in the above Item 7.

[0037] Utility Model Effect

[0038] The utility model achieves the following effects.

[0039] In the above 1, the outer adhesive layer contains an insulating reinforcing agent, thereby, compared with an outer adhesive layer not containing an insulating reinforcing agent, the insulating property of the outer adhesive layer is improved, and the outer adhesive layer is less likely to break, and the breaking strength (tensile breaking strength, etc.) and elongation at break (tensile breaking elongation, etc.) of the outer adhesive layer are improved. Therefore, the insulating property and puncture strength of the packaging material can be improved.

[0040] Therefore, even if the outer surface of the packaging material is damaged by cracks, scratches, etc., for example due to severe deformation of the packaging material caused by molding or contact between a protrusion and the outer surface of the packaging material, the reduction in the insulation properties of the packaging material caused by the damage can be suppressed.

[0041] In the above Item 2, the number average particle size of the insulation reinforcing particles as the insulation reinforcing agent is in the range of 0.01 μm to 3 μm, thereby lengthening the fracture path in the outer adhesive layer, further improving the fracture strength and elongation at break of the outer adhesive layer, and thus further improving the puncture strength of the packaging material.

[0042] In the above Item 3, the specific surface area of ​​the insulation enhancing particles is 1 m 2 / g or more, the interaction between the insulation-enhancing particles and the outer adhesive molecules is reliably increased, and the breaking strength of the outer adhesive layer is reliably improved. Therefore, the puncture strength of the packaging material can be reliably improved.

[0043] In the above 4, the volume resistivity of the insulating reinforcing particles is 1×10 12 Ωcm or more, thereby making it possible to reliably improve the insulation properties of the outer adhesive layer.

[0044] In the above Item 5, the tensile elongation at break L of the cured film of the outer adhesive composition satisfies the above Relationship 1, whereby the outer adhesive layer in the packaging material has high followability to the deformation of the metal foil layer, thereby reliably improving the puncture strength of the packaging material.

[0045] In the above item 6, the outer adhesive layer is 2g / m 2 ~10g / m 2The coating amount in the range of is set between the metal foil layer and the heat-resistant resin layer, and the content of the insulating reinforcing agent in the outer adhesive layer is 0.2g / m 2 ~1.0g / m 2 In the range of , the breaking strength and breaking elongation of the outer adhesive layer are reliably improved. Therefore, the puncture strength of the packaging material can be reliably improved.

[0046] In the aforementioned item 7, a packaging case having high puncture strength and high insulation properties can be provided.

[0047] In the aforementioned Item 8, the power storage device includes the package case described in the aforementioned Item 7, and therefore has high durability against external forces such as impact, vibration, and external pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a schematic cross-sectional view of a molding packaging material according to one embodiment of the present invention.

[0049] Figure 2 This is a schematic cross-sectional view of a power storage device according to one embodiment of the present invention.

[0050] Figure 3 It is a schematic perspective view showing the power storage device in an exploded state.

[0051] Figure 4 This is a diagram for explaining a method for measuring the volume resistivity of insulation-reinforcing particles.

[0052] Description of Reference Numerals

[0053] 1: Packaging materials

[0054] 2: Metal foil layer

[0055] 3: Heat-resistant resin layer

[0056] 4: Thermally fusible resin layer

[0057] 5R: Outer adhesive layer

[0058] 6: Inner adhesive layer

[0059] 30: Lithium-ion battery (power storage device)

[0060] 31: Lithium-ion battery main body (power storage device main body) DETAILED DESCRIPTION

[0061] An embodiment of the present invention is described below with reference to the accompanying drawings.

[0062] like Figure 1 As shown in FIG. 1 , a molding packaging material 1 according to an embodiment of the present invention includes an inner surface 1 a and an outer surface 1 b .

[0063] The packaging material 1 is basically formed of a laminated body including a metal foil layer 2, a heat-resistant resin layer 3 disposed on the outer surface side of the metal foil layer 2, and a heat-fusible resin layer 4 disposed on the inner surface side of the metal foil layer 2 in a laminated state, an outer adhesive layer 5R is provided between the metal foil layer 2 and the heat-resistant resin layer 3, and an inner adhesive layer 6 is provided between the metal foil layer 2 and the heat-fusible resin layer 4. These layers are joined (bonded) and integrated in a laminated state.

[0064] The heat-fusible resin layer 4 is disposed on the inner surface 1a of the packaging material 1, and thus the inner surface 1a of the packaging material 1 is formed by the inner surface of the heat-fusible resin layer 4. The heat-resistant resin layer 3 is also called the base material layer of the packaging material 1 and is disposed on the outer surface 1b side of the metal foil layer 2 of the packaging material 1.

[0065] A chemical conversion film 2a for improving the corrosion resistance of the metal foil layer 2 is formed on at least one of the inner surface and the outer surface of the metal foil layer 2. In the present embodiment, chemical conversion films 2a and 2a are formed on the inner surface and the outer surface of the metal foil layer 2, respectively. Each chemical conversion film 2a is formed by subjecting the surface of the metal foil to a chemical conversion treatment.

[0066] The packaging material 1 may be Figure 2 and 3 The packaging shown is used for a power storage device such as a battery device. Specifically, the power storage device is a lithium ion battery 30, for example.

[0067] like Figure 3 As shown, a lithium-ion battery 30 as an electric storage device includes a lithium-ion battery body 31 as the main body of the electric storage device, and a package case 20 that accommodates the battery body 31 in a state of surrounding the battery body 31. The package case 20 includes a container-shaped package case body 21 opened at the top, and a flat plate-shaped cover body 22 that closes the opening of the package case body 21 as components of the package case 20.

[0068] The package case body 21 is formed by deep drawing or stretching the packaging material 1 into a container shape with its inner surface 1a facing inward.

[0069] A recess 21b for housing the battery body 31 is provided at the center of the inner surface 1a of the package case body 21. A flange 21a protruding outward is provided at the upper end of a side wall 21c disposed on the outer periphery of the package case body 21 as a predetermined joining portion.

[0070] The cover body 22 is a cover body used in a flat state without the packaging material 1 being subjected to molding, and an outer peripheral portion 22 a of the cover body 22 is a predetermined joining portion of the cover body 22 .

[0071] In the battery 30, the battery body 31 is accommodated and arranged in the recess 21b of the package case body 21, and the cover body 22 is arranged on the package case body 21 in such a manner that the inner surface 1a thereof faces the battery body 31 side (lower side), and the heat-fusible resin layer 4 of the flange portion 21a of the package case body 21 and the heat-fusible resin layer 4 of the outer peripheral portion 22a of the cover body 22 are heat-fused (joined) in a sealed state by heat sealing, thereby forming a structure as shown in FIG. Figure 2 As shown, the battery 30 is in a state where the battery main body 31 is accommodated in the packaging case 20 .

[0072] It should be noted that Figure 2 Reference numeral “ 23 ” in the figure denotes a heat-sealed portion (heat-welded portion) between the heat-weldable resin layer 4 of the flange portion 21 a of the package case body 21 and the heat-weldable resin layer 4 of the outer peripheral portion 22 a of the lid body 22 .

[0073] The tab (not shown) connected to the battery body 31 is usually led out from the battery body 31 to the outside of the package case 20 through the heat-sealed portion 23 .

[0074] Next, the configuration of the packaging material 1 and the method for producing the packaging material 1 according to the present embodiment will be described in detail below.

[0075] (Heat-resistant resin layer)

[0076] The heat-resistant resin layer 3 is formed of, for example, a heat-resistant resin film. The type of the heat-resistant resin layer (heat-resistant resin film) 3 is not limited. As the heat-resistant resin layer 3, polyamide film, polyester film, etc. can be used, and their stretched films are preferably used. Among them, as the heat-resistant resin layer 3, from the aspects of excellent molding processability and strength, biaxially stretched polyamide film, biaxially stretched polybutylene terephthalate (PBT) film, biaxially stretched polyethylene terephthalate (PET) film or biaxially stretched polyethylene naphthalate (PEN) film is preferably used.

[0077] In addition, biaxially stretched polyamide films are particularly preferably used as the heat-resistant resin layer 3 in view of excellent puncture strength and molding processability. The type of polyamide film is not limited, and examples of the polyamide film include nylon 6 film, nylon 6,6 film, nylon MXD film, and the like.

[0078] The heat-resistant resin layer 3 may be formed of a single layer, or may be formed of a multilayer including, for example, a PET film / polyamide film.

[0079] The thickness of the heat-resistant resin layer 3 is not limited, but is preferably in the range of 9 μm to 50 μm. When a polyester film is used as the heat-resistant resin layer 3, the thickness is preferably in the range of 9 μm to 50 μm, and when a polyamide film is used, the thickness is preferably in the range of 10 μm to 50 μm. By making the thickness greater than the lower limit of the above-mentioned preferred range, it is possible to reliably ensure strength sufficient for the packaging material 1, and by making the thickness less than the upper limit of the above-mentioned preferred range, it is possible to reliably reduce the processing stress acting on the packaging material 1 during deep drawing and stretching, and the molding processability of the packaging material 1 can be reliably improved.

[0080] When the heat-resistant resin layer 3 is formed of multiple layers, the thickness thereof is preferably in the range of 20 μm to 50 μm. For example, when the heat-resistant resin layer 3 is formed of multiple layers including PET film / polyamide film, it is preferred that the multiple layers are formed by laminating the two films by dry lamination using the same adhesive as the outer adhesive layer 5R.

[0081] (Thermal Fusible Resin Layer)

[0082] The heat-fusible resin layer 4 is a layer that plays the role of providing the packaging material 1 with excellent chemical resistance to highly corrosive electrolytes used in the power storage device 30 such as lithium ion batteries and imparting heat sealability to the packaging material 1 .

[0083] The heat-fusible resin layer 4 is formed of, for example, a heat-fusible resin film. The type of the heat-fusible resin layer (heat-fusible resin film) 4 is not limited, and as the heat-fusible resin layer 4, a heat-fusible resin unstretched film can be preferably used. As the heat-fusible resin unstretched film, from the perspective of excellent chemical resistance and heat sealing properties, it is preferred to use an unstretched film formed of at least one heat-fusible resin selected from the group consisting of polyethylene, polypropylene, olefin copolymers, their acid-modified products, and ionomers. In particular, from the perspective of excellent puncture strength, it is preferred to use a three-layer co-extruded polypropylene film in which a coating layer containing a random copolymer polypropylene is laminated and integrated on both sides of an intermediate layer containing a block copolymer polypropylene. It should be noted that the layer thickness ratio of the unstretched three-layer co-extruded polypropylene film is not limited, and is preferably in the range of ethylene-propylene random copolymer (rPP): ethylene-propylene block copolymer (bPP): ethylene-propylene random copolymer (rPP) = 1 to 1.5: 7 to 8: 1 to 1.5.

[0084] The thickness of the heat-fusible resin layer 4 is not limited, but is preferably in the range of 20 μm to 80 μm. By making the thickness 20 μm or more, the generation of pinholes in the molded product can be reliably suppressed. By making the thickness 80 μm or less, the amount of resin used can be reliably reduced, and the manufacturing cost of the packaging material 1 can be reliably reduced. Among them, the thickness of the heat-fusible resin layer 4 is particularly preferably in the range of 30 μm to 50 μm.

[0085] (Metal foil layer)

[0086] The metal foil layer 2 is a layer that plays a role in providing the packaging material 1 with gas barrier properties for suppressing the intrusion of oxygen and moisture.

[0087] The metal foil layer 2 is formed of, for example, a metal foil. The type of the metal foil layer 2 is not limited, and aluminum foil, copper foil, stainless steel foil, etc. can be used as the metal foil layer 2, and aluminum foil is usually used. As the aluminum foil, an Al-Fe alloy foil containing 0.7 mass % to 1.7 mass % of Fe in particular has excellent strength and ductility, and can obtain good molding processability.

[0088] The thickness of the metal foil layer 2 is not limited, and can preferably be in the range of 20 μm to 100 μm. By making the thickness greater than 20 μm, the generation of pinholes can be reliably suppressed during rolling when manufacturing the metal foil. By making the thickness less than 100 μm, the processing stress acting on the packaging material 1 during deep drawing and stretching can be reliably reduced, and the formability of the packaging material 1 can be reliably improved.

[0089] (Chemical conversion coating of metal foil layer)

[0090] The chemical conversion film 2a is a film (layer) for improving the corrosion resistance of the metal foil layer 2, and can be formed, for example, by subjecting the surface of the metal foil constituting the metal foil layer 2 to a chromate treatment or a non-chromium type chemical conversion treatment using a zirconium compound or the like. For example, in the case of a chromate treatment, an aqueous solution of any one of the following mixtures 1) to 3) is applied to the surface of the metal foil subjected to a degreasing treatment and then dried.

[0091] 1) A mixture of phosphoric acid, chromic acid, and at least one of a metal salt of fluoride and a non-metal salt of fluoride

[0092] 2) A mixture of any one of an acrylic resin, a chitosan derivative resin and a phenolic resin, at least one of chromic acid and a chromium (III) salt, and phosphoric acid

[0093] 3) A mixture of any one of an acrylic resin, a chitosan derivative resin and a phenolic resin, at least one of chromic acid and a chromium (III) salt, at least one of a metal salt of fluoride and a non-metal salt of fluoride, and phosphoric acid.

[0094] The amount of chromium deposited in the chemical conversion film 2a is not limited, but is preferably 0.1 mg / m2 on one side of the metal foil. 2 ~50 mg / m 2 The range is particularly preferably 2 mg / m 2 ~20 mg / m 2 The thickness of the chemical conversion film 2a is not limited, but is preferably in the range of 0.001 μm to 0.1 μm. Due to the chemical conversion film 2a having such a chromium deposition amount or thickness, the corrosion resistance of the metal foil layer 2 can be reliably improved.

[0095] In the present embodiment, the chemical conversion film 2 a is formed on the inner surface and the outer surface of the metal foil layer 2 as described above. However, in the present invention, the chemical conversion film 2 a may be formed on only one of the inner surface and the outer surface of the metal foil layer 2 .

[0096] (Outer adhesive layer)

[0097] The outer adhesive layer 5R is a layer responsible for the bonding between the metal foil layer 2 and the layer arranged on the outer surface side of the metal foil layer 2. In the present embodiment, it is a layer responsible for the bonding between the metal foil layer 2 (specifically, the outer surface chemical conversion film 2a of the metal foil layer 2) and the heat-resistant resin layer 3.

[0098] The outer adhesive layer 5R is formed of a cured film of an outer adhesive composition containing an outer adhesive and an insulation reinforcing agent.

[0099] Hereinafter, in order to distinguish the above-mentioned outer adhesive composition containing an outer adhesive and an insulation reinforcing agent from the outer adhesive composition containing an outer adhesive but not containing an insulation reinforcing agent, the former is also referred to as "an outer adhesive composition containing an insulation reinforcing agent", and the latter is referred to as "an outer adhesive composition not containing an insulation reinforcing agent". Therefore, in the present embodiment, the outer adhesive layer 5R is formed of a cured film of the outer adhesive composition containing an insulation reinforcing agent.

[0100] The type of the external adhesive is not limited, and the external adhesive may include polyurethane adhesives, acrylic adhesives, polyacrylate adhesives, modified polypropylene adhesives, polyester adhesives, polyamide adhesives, epoxy adhesives, etc. Among them, polyurethane adhesives are preferably used.

[0101] In addition, the outer adhesive is preferably an adhesive that can be used as an adhesive for dry lamination (for example, a urethane adhesive, an olefin adhesive). Specifically, as such an outer adhesive, for example, an adhesive containing a two-component curing polyester urethane resin formed of a polyester resin as a main agent of the outer adhesive and a polyfunctional isocyanate compound as a curing agent can be used.

[0102] The method for bonding the metal foil layer 2 and the heat-resistant resin layer 3 with the outer adhesive composition is not limited, and an example thereof is a dry lamination method.

[0103] As the insulation enhancing agent, insulation enhancing particles can be used. As the insulation enhancing particles, at least one of insulating inorganic particles and organic particles can be used. It should be noted that, generally, organic particles have insulating properties.

[0104] As insulating inorganic particles, for example, fillers listed in "Table 1 Types and properties of fillers" in "Reinforcement (One) Inorganic Reinforcers" by Shiraki Yoshikazu, Journal of the Rubber Association of Japan, Vol. 53, No. 1, pp. 17-33, 1980, can be used. Specifically, as insulating inorganic particles, at least one particle selected from the group consisting of calcium carbonate (CaCO3), magnesium carbonate, calcium / magnesium carbonate, silicate, silicon dioxide (silicic acid: SiO2), aluminum hydrate, barium sulfate, calcium sulfate and calcium sulfite is preferably used.

[0105] As the organic particles, it is preferable to use particles (beads) of at least one selected from the group consisting of acrylic resin, styrene resin, and fluororesin.

[0106] Therefore, as the insulating reinforcing particles, at least one selected from the group consisting of the above-mentioned insulating inorganic particles and the above-mentioned organic particles is preferably used. In addition, the insulating inorganic particles and the organic particles may also be mixed and used. In particular, as the insulating inorganic particles, at least one selected from the group consisting of silicon dioxide and calcium carbonate is preferably used. In addition, in particular, as the organic particles, acrylic resin particles are preferably used.

[0107] By making the outer adhesive layer 5R contain insulating reinforcing particles as an insulating reinforcing agent, the insulating property of the outer adhesive layer 5R is improved compared with the outer adhesive layer not containing the insulating reinforcing agent, and the outer adhesive layer 5R is not easily broken, and the breaking strength (tensile breaking strength, etc.) and elongation at break (tensile breaking elongation, etc.) of the outer adhesive layer 5R are improved. Therefore, the insulating property and puncture strength of the packaging material 1 can be improved.

[0108] Therefore, even in the case where the outer surface 1b of the packaging material 1 is damaged by cracks, scratches, etc., for example, due to severe deformation of the packaging material 1 caused by molding processing or contact between a protrusion and the outer surface 1b of the packaging material 1, the reduction in the insulation properties of the packaging material 1 caused by the damage can be suppressed.

[0109] The number average particle size of the insulating reinforcing particles (insulating reinforcing agent) is preferably small, and may more preferably be in the range of 0.01 μm to 3 μm. In this case, the fracture path in the outer adhesive layer 5R becomes longer, and the fracture strength and elongation at break of the outer adhesive layer 5R are further improved. Therefore, the puncture strength of the packaging material 1 can be further improved. In addition, by making the number average particle size of the insulating reinforcing particles greater than 0.01 μm, the hardening of the outer adhesive layer 5R due to the inclusion of insulating reinforcing particles can be suppressed. By making the number average particle size of the insulating reinforcing particles less than 3 μm, the reinforcing effect of the outer adhesive layer 5R brought about by the inclusion of insulating reinforcing particles can be reliably obtained. The more preferred upper limit of the number average particle size of the insulating reinforcing particles is 2.0 μm.

[0110] The specific surface area of ​​the insulation-enhancing particles is preferably large, and may be preferably 1 m 2 In this case, the interaction between the insulating reinforcing particles and the outer adhesive molecules is reliably increased, and the breaking strength of the outer adhesive layer 5R is reliably improved. Therefore, the puncture strength of the packaging material 1 can be reliably improved. The more preferred lower limit of the specific surface area of ​​the insulating reinforcing particles is 10 m 2 The upper limit of the specific surface area of ​​the insulating reinforcing particles is preferably 500 m 2 / g. If the specific surface area is greater than 500m 2 / g, the interaction between the reinforcing particles and the outer adhesive molecules is saturated, and the improvement of the breaking strength of the outer adhesive layer 5R is not observed. Therefore, the specific surface area is preferably 500m 2 / g or less. A further preferred upper limit is 450m 2 / g, and the upper limit is particularly preferably 350m 2 / g.

[0111] The volume resistivity of the insulating reinforcing particles is preferably equal to or greater than the volume resistivity of a cured film of an adhesive used as an external adhesive. Specifically, it is preferably 1×10 12 That is, since the volume resistivity of the cured film of the adhesive generally used as the outer adhesive is 1×10 11 Ωcm or more, therefore, by making the volume resistivity of the insulation-enhancing particles 1×10 12Ωcm or more, the insulation of the outer adhesive layer 5R can be reliably improved. The more preferred lower limit of the volume resistivity of the insulation reinforcing particles is 1×10 13 Ωcm, and a further preferred lower limit is 1×10 14 The more preferred upper limit of the volume resistivity of the insulating reinforcing particles is 1×10 16 Ωcm.

[0112] For reference, some examples of volume resistivity of cured films of adhesives (resins) generally used as external adhesives are described below.

[0113] Urethane resin (assumed as outer adhesive layer): 1×10 11 ~1×10 13 Ωcm

[0114] Acrylic resin (methacrylic resin): ≥1×10 14 Ωcm

[0115] Polyester resin: 1×10 15 ~1×10 16 Ωcm

[0116] Polypropylene resin: ≥1×10 16 Ωcm

[0117] Polyamide resin (polyamide 6): 1×10 11 Ωcm.

[0118] Furthermore, for reference, the volume resistivity of silica particles, calcium carbonate particles, titanium oxide particles, and carbon black is described below.

[0119] Silica particles (SiO2 particles): 1×10 16 Ωcm

[0120] Calcium carbonate particles (CaCO3 particles): 1×10 14 Ωcm

[0121] Titanium oxide particles (TiO2 particles): 1×10 4 ~1×10 11 Ωcm

[0122] Carbon black: 1×10 -2 ~1×10 -1 Ωcm.

[0123] Among silica particles, calcium carbonate particles, titanium oxide particles and carbon black, the volume resistivity is 1×10 12Particles with a diameter of Ωcm or more are silica particles and calcium carbonate particles. Therefore, it is particularly preferable to use at least one of silica particles and calcium carbonate particles as the insulation-reinforcing particles.

[0124] In the insulation reinforcing agent (insulation reinforcing particles), functional groups can be added by subjecting the insulation reinforcing agent to a silane-based or titanium-based coupling agent treatment or a surface treatment based on a synthetic polymer, etc. In this case, the surface activity of the insulation reinforcing agent can be increased, thereby improving the interfacial adhesion between the insulation reinforcing agent and the external adhesive.

[0125] Preferred conditions for the outer adhesive composition containing the insulation enhancing agent are as follows.

[0126] The content of the insulating enhancer relative to the total amount of the insulating enhancer and the main agent of the outer adhesive is preferably in the range of 2 mass % to 10 mass %. It should be noted that, in detail, the content refers to the solid content, that is, the content does not include the mass of the solvent. The following are the same.

[0127] The outer adhesive layer 5R is preferably 2 g / m 2 ~10g / m 2 The coating amount in the range of is provided between the metal foil layer 2 and the heat-resistant resin layer 3. In addition, the content of the insulating reinforcing agent in the outer adhesive layer 5R is preferably 0.2 g / m 2 ~1.0g / m 2 By making the coating amount of the outer adhesive layer 5R within the above range and the content of the insulating enhancer within the above range, the breaking strength and breaking elongation of the outer adhesive layer 5R are reliably improved. Therefore, the puncture strength of the packaging material 1 can be reliably improved, and the molding processability of the packaging material 1 can also be reliably improved. It should be noted that the coating amount of the outer adhesive layer 5R mentioned above refers to the solid component coating amount in detail, and the content of the insulating enhancer mentioned above refers to the solid component content in detail. The following are the same.

[0128] The more preferred lower limit of the coating amount of the outer adhesive layer 5R is 4 g / m 2 The more preferred upper limit is 9 g / m 2 The more preferred range of the content of the above-mentioned insulating enhancer is 0.2 g / m 2 ~0.7g / m 2 .

[0129] The method for laminating (bonding) the metal foil layer 2 and the heat-resistant resin layer 3 is not limited, but dry lamination is preferred.

[0130] When the tensile elongation at break of a cured film of an outer adhesive composition containing an insulation reinforcing agent is L and the tensile elongation at break of a cured film of an outer adhesive composition containing no insulation reinforcing agent is L0, L preferably satisfies the following relational expression 1.

[0131] 15%≤{(L-L0) / L0}×100%≤250%…(Formula 1).

[0132] When L satisfies the above-mentioned relational expression 1, the outer adhesive layer 5R has high followability to the deformation of the metal foil layer 2 in the packaging material 1. Therefore, the puncture strength of the packaging material 1 can be reliably improved, and the molding processability of the packaging material 1 can also be reliably improved.

[0133] In the above relational expression 1, {(L-L0) / L0}×100% as the middle side thereof refers to the improvement rate ΔL of the tensile elongation at break of the cured film of the outer adhesive composition (outer adhesive layer 5R) achieved by containing the insulating reinforcing agent (i.e., ΔL={(L-L0) / L0}×100%). Even if the improvement rate ΔL is greater than 250%, the improvement in the puncture strength and molding processability of the packaging material 1 is not much observed. The improvement rate ΔL is particularly preferably in the range of 20% to 230%, and even more preferably in the range of 50% to 230%.

[0134] When dispersing the insulation reinforcing agent in the outer adhesive in order to make the insulation reinforcing agent contained in the outer adhesive, it is preferable to use a disperser for dispersion. In addition, a dispersant such as a surfactant may be used for the dispersion.

[0135] The method for dispersing the insulating reinforcing agent in the outer adhesive is not limited, but the following method is preferable.

[0136] That is, an ink containing an insulation enhancer at a high concentration (also referred to as "ink containing a high concentration insulation enhancer") is prepared in advance. Then, the ink is added to an external adhesive (preferably a main agent of the external adhesive) so that the content of the insulation enhancer becomes a predetermined ratio and mixed, thereby dispersing the insulation enhancer in the external adhesive (its main agent).

[0137] The ink can be prepared, for example, as follows.

[0138] That is, an insulating enhancer is added to a varnish (a mixture of a resin and a solvent) and mixed to prepare a base of ink, to which auxiliary agents (surfactants, viscosity regulators, antistatic agents, antioxidants, dispersants, leveling agents, anti-settling agents, defoaming agents, etc.) are added, and a disperser is used for mixing and dispersing, thereby uniformly dispersing the insulating enhancer in the varnish, thereby preparing the above-mentioned ink containing a high concentration of the insulating enhancer.

[0139] As the resin for the varnish, one or a combination of two or more selected from the group consisting of a copolymer of vinyl chloride and vinyl acetate, chlorinated rubber, chlorinated polypropylene, acrylic resin, polyamide resin, polyurethane resin, polyester resin and nitrocellulose can be used. In particular, as the resin, it is preferred to use a resin of the same type (more preferably the same composition) as the main agent of the external adhesive, thereby making the ink and the main agent of the external adhesive easily compatible (mixable).

[0140] As the paint solvent, one or a combination of two or more selected from the group consisting of toluene, methyl ethyl ketone, methylcyclohexane, ethyl acetate and isopropyl alcohol can be used. In particular, ethyl acetate, which can also be used as a solvent for the outer adhesive, is preferably used as the solvent. In addition, toluene, methyl ethyl ketone, etc. can be used as a cosolvent as needed.

[0141] As the insulating reinforcing agent, it is preferable to use at least one of the above-mentioned insulating inorganic particles and the above-mentioned organic particles.

[0142] The ink is preferably prepared using a paint resin, a paint solvent, an insulation enhancer, and an auxiliary agent in the following blending ratio.

[0143] Resin: 15% to 25% by mass

[0144] Solvent: 40% to 70% by mass

[0145] Insulation enhancer: 5% to 50% by mass

[0146] Auxiliary agent: 1% to 5% by mass.

[0147] In addition, the insulating enhancer is preferably dispersed in the ink at a high concentration and uniformly. In order to prepare such an ink, as the above-mentioned disperser, a paint shaker, a ball mill, a grinder, a sand mill, a bead mill, a Dynomill, a roller mill, an ultrasonic grinder, a high-pressure collision disperser, etc. can be used. In addition, one disperser can be used for one or more dispersion treatments, or two or more dispersers can be used in combination for multiple dispersion treatments.

[0148] As described above, by adding the ink containing the insulating enhancer at a high concentration to the outer adhesive (preferably the main agent of the outer adhesive) so that the content of the insulating enhancer becomes a predetermined ratio, and uniformly mixing and dispersing, it is possible to reliably suppress the insulating enhancer from generating secondary aggregated particles, thereby reliably making the insulating enhancer uniformly dispersed in the outer adhesive (its main agent). Thus, it is possible to reliably obtain the outer adhesive (its main agent) in which the insulating enhancer is well dispersed, such that the insulating enhancer does not precipitate even if the insulating enhancer is added to the outer adhesive (its main agent) and left for several months.

[0149] When the insulating enhancer is added to the main agent of the outer adhesive, for example, the main agent of the outer adhesive obtained as described above and well dispersed with the insulating enhancer is reacted with a curing agent (for example, an isocyanate curing agent), and a cured film of the outer adhesive composition (i.e., the outer adhesive layer 5R) with very few coating defects caused by the secondary agglomerated particles of the insulating enhancer can be reliably formed. Thus, the tensile elongation at break L of the cured film is reliably improved compared to the cured film of the outer adhesive composition not containing the insulating enhancer, and the cured film of the outer adhesive composition can reliably follow the deformation and puncture deformation during the molding process. Therefore, the outer adhesive layer 5R can reliably maintain good adhesion.

[0150] (Inner adhesive layer)

[0151] The inner adhesive layer 6 has an adhesive component such as an adhesive agent or adhesive resin interposed between the metal foil layer 2 and the thermally adhesive resin layer 4 and is a layer that joins (bonds) the metal foil layer 2 and the thermally adhesive resin layer 4 in a laminated state via the adhesive component.

[0152] Here, in order to easily distinguish the above-mentioned adhesive, adhesive resin and adhesive component from the above-mentioned outer adhesive, they are hereinafter also referred to as "inner adhesive", "inner adhesive resin" and "inner adhesive component", respectively.

[0153] As the inner adhesive, for example, the same adhesive as the outer adhesive used in the outer adhesive layer 5R described above may be used, or a different adhesive may be used.

[0154] As the inner adhesive resin, one of polyolefin resins, polyvinyl acetate resins, (meth) acrylic resins, amino resins, etc. can be used alone, or two or more can be used in combination. It should be noted that, as the above-mentioned polyolefin resins, polyolefin resins, carboxylic acid-modified polyolefin resins, metal-modified polyolefin resins, etc. can be cited.

[0155] When the metal foil layer 2 and the heat-fusible resin layer 4 are joined (bonded) using an inner adhesive, a dry lamination method can be used as a joining method, and the method is as follows.

[0156] That is, on the metal foil layer 2 or the heat-fusible resin layer 4, the inner adhesive composition is applied in layers by gravure coating, reverse roll coating, etc., and the solvent in the composition is dried and evaporated to form a dry film, and then the metal foil layer 2 and the heat-fusible resin layer 4 are attached. Then, the composition is cured according to the curing conditions of the composition. Thus, the metal foil layer 2 and the heat-fusible resin layer 4 are joined (bonded) in a laminated state via the inner adhesive layer 6.

[0157] When the metal foil layer 2 and the heat-fusible resin layer 4 are joined (bonded) in a laminated state using the inner adhesive resin, the following three methods can be used as the joining method, for example.

[0158] That is, the following methods can be used: a method of co-extruding an inner adhesive resin and a hot-melt adhesive resin on the metal foil layer 2 (specifically, the inner surface of the metal foil layer 2) to thereby join the metal foil layer 2 and the hot-melt adhesive resin layer 4 in a laminated state (coextrusion lamination method); a method of pre-forming a laminated body in which the inner adhesive resin and the hot-melt adhesive resin are laminated, laminating the laminated body on the metal foil layer 2 by a hot lamination method, and joining the laminated body; and a method of laminating the metal foil layer 2 and the hot-melt adhesive resin in a film form while flowing a molten inner adhesive resin between the metal foil layer 2 and the hot-melt adhesive resin in a film form (sandwich lamination method).

[0159] (Method for producing packaging material)

[0160] An example of a preferred method for producing the packaging material 1 is as follows.

[0161] A metal foil layer 2 having chemical conversion films 2a formed on the inner and outer surfaces is prepared. Next, an outer adhesive composition containing an insulation reinforcing agent is applied in a layer to the outer surface of the metal foil layer 2 by a predetermined coating method, and the solvent in the composition is dried and evaporated. Then, the outer surface of the metal foil layer 2 is bonded to the inner surface of the heat-resistant resin layer 3, and the composition is cured by being maintained (aged) at a predetermined temperature according to the curing conditions of the composition.

[0162] Next, a state is created in which the hot-melt adhesive resin layer 4 is bonded to the inner surface of the metal foil layer 2 via an inner adhesive component (inner adhesive, inner adhesive resin, etc.), and the inner adhesive component is cured by being maintained (aged) at a specified temperature according to the curing conditions of the inner adhesive component.

[0163] Thus, the heat-resistant resin layer 3 is bonded to the outer surface of the metal foil layer 2 via the outer adhesive layer 5R, and the thermally fusible resin layer 4 is bonded to the inner surface of the metal foil layer 2 via the inner adhesive layer 6, thereby obtaining the packaging material 1.

[0164] However, the packaging material according to the present invention is not limited to the packaging material manufactured by the above-mentioned method for manufacturing the packaging material 1, and may be a packaging material manufactured by other methods.

[0165] As mentioned above, although embodiment of this invention is described, this invention is not limited to the said embodiment, Various changes can be made within the range which does not deviate from the summary of this invention.

[0166] For example, the packaging material of the present invention is not limited to Figure 1 The packaging material of the multiple layers shown can also be, for example, Figure 1 A packaging material in which a new layer is added to the plurality of layers shown to increase or improve the function of the packaging material.

[0167] Example

[0168] Specific examples and comparative examples of the present invention are shown below. However, the present invention is not limited to the following examples.

[0169] Here, in the following Examples 1 to 10 and the following Comparative Examples 1 to 2, aluminum foil of the same material is used as the metal foil layer 2. The material is aluminum alloy symbol A8079 specified by JIS H4160. The thickness of all aluminum foils is 35 μm. In addition, chemical conversion coatings 2a obtained by the same chemical conversion treatment as in Example 1 are formed on the inner and outer surfaces of all aluminum foils.

[0170] In addition, in the following Examples 1 to 10 and the following Comparative Examples 1 to 2, the same monolayer biaxially stretched nylon (ONY) film was used as the heat-resistant resin layer 3. The thickness of all the films was 15 μm. In addition, the inner surface of all the films (i.e., the bonding surface with the metal foil layer 2 in the film) was pre-corona treated in order to improve the wettability with the outer adhesive composition.

[0171] In the following Examples 1 to 10 and Comparative Examples 1 to 2, the same unstretched three-layer coextruded polypropylene (CPP) film was used as the heat-fusible resin layer 4. The thickness of all the films was 30 μm, and the layer thickness ratio was rPP:bPP:rPP=1:8:1. In addition, the outer surface of all the films (i.e., the surface of the film that is bonded to the metal foil layer 2) was pre-corona treated in order to improve the wettability with the inner adhesive component.

[0172] In Examples 1 to 5 and Comparative Example 1, the metal foil layer 2 and the heat-fusible resin layer 4 were bonded by dry lamination, and in Examples 6 to 10 and Comparative Example 2, the metal foil layer 2 and the heat-fusible resin layer 4 were bonded by sandwich lamination.

[0173] <Example 1>

[0174] A chemical conversion film 2a is formed on the inner and outer surfaces of the aluminum foil as the metal foil layer 2. The chemical conversion film 2a is formed by applying a chemical conversion treatment solution composed of polyacrylic acid, a trivalent chromium compound, water and an alcohol to the inner and outer surfaces of the aluminum foil and then drying at 150°C. The chromium deposition amount of the chemical conversion film 2a is 10 mg / m2 on one side of the aluminum foil. 2 The thickness of each chemical conversion film 2a is 0.01 μm.

[0175] The above-mentioned biaxially stretched nylon (ONY) film was prepared as the heat-resistant resin layer 3. The TD hot water shrinkage of the film was 2.7%, the MD hot water shrinkage was 2.0%, the difference in hot water shrinkage between TD and MD (TD-MD) was 0.7%, the TD elastic modulus was 1.7 GPa, the MD elastic modulus was 2.7 GPa, the TD breaking strength was 361 MPa, the MD breaking strength was 280 MPa, and the number average molecular weight of the polyamide was 25,000.

[0176] As the outer adhesive composition constituting the outer adhesive layer, first, an outer adhesive composition containing an outer adhesive but not containing an insulation reinforcing agent, that is, an outer adhesive composition not containing an insulation reinforcing agent is prepared. In the outer adhesive composition, a two-component curing polyester urethane resin is used as the outer adhesive. The preparation method of the outer adhesive composition is as follows.

[0177] First, a polyester resin (polyester polyol) as the main agent of a two-liquid curable polyester urethane resin was prepared by the following method. That is, 30 mol parts of neopentyl glycol, 30 mol parts of ethylene glycol, and 40 mol parts of 1,6-hexanediol were melted at 80°C, and the melt was subjected to a condensation reaction at 210°C for 20 hours with stirring with 30 mol parts of adipic acid (methylene number is 4) as an aliphatic dicarboxylic acid and 70 mol parts of isophthalic acid as an aromatic dicarboxylic acid, thereby obtaining a polyester polyol as the main agent. The number average molecular weight (Mn) of the polyester polyol is 12,000, the weight average molecular weight (Mw) is 20,500, and their ratio (Mw / Mn) is 1.7. Furthermore, 60 parts by mass of ethyl acetate are added to 40 parts by mass of the polyester polyol to prepare a flowing polyester polyol resin solution. Its hydroxyl value is 2.2 mgKOH / g (solution value).

[0178] Next, 7.1 parts by mass of an adduct of toluene diisocyanate (TDI) (aromatic) and trimethylolpropane (TMP) (NCO: 13.0% by mass, solid content: 75% by mass) as a curing agent was added to 100 parts by mass of the polyester polyol resin solution as the main agent, and 34.1 parts by mass of ethyl acetate was further added, and stirred and mixed to prepare an outer adhesive composition (i.e., a two-component curable polyester urethane resin) not containing an insulation enhancer. In the outer adhesive composition, the molar ratio (-NCO) / (-OH) of the isocyanate functional group (-NCO) to the polyester polyol hydroxyl group (-OH) was 10.

[0179] Next, a cured film of the outer adhesive composition was prepared by the following method, and its physical properties were evaluated.

[0180] That is, the outer adhesive composition is applied in a layer on a non-adhesive untreated polypropylene film so that the thickness after drying is 10 μm, the solvent in the composition is dried and evaporated, and then the composition is aged at 60° C. until the residual isocyanate is 5% by mass or less, thereby curing. Then, the cured product is peeled off from the untreated polypropylene film, thereby preparing a cured film (10 μm thick) of the outer adhesive composition.

[0181] The cured film was cut into 15 mm width to collect a test piece, and then the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L0 of the test piece. As a result, the tensile breaking strength was 30 MPa and the tensile breaking elongation L0 was 18%.

[0182] It should be noted that the above-mentioned tensile test was conducted under the conditions of a point distance of 50 mm and a tensile speed of 100 mm / min in accordance with JIS K7161-1:2014. The following are the same.

[0183] Next, a polyester resin (polyester polyol) containing a two-component curing polyester urethane resin as a main component and silicon dioxide particles (SiO2 particles: number average particle size of 0.4 μm, specific surface area of ​​10 m 2 / g, volume resistivity is 1×10 16 Ωcm) of the outside adhesive composition, that is, the outside adhesive composition containing the insulation enhancing agent. The preparation method of the composition is as follows.

[0184] 20 parts by mass of the polyester polyol as a paint resin, 40 parts by mass of ethyl acetate as a paint solvent, 35 parts by mass of the silica particles as an insulation enhancer, and 5 parts by mass of auxiliary agents (dispersant and anti-settling agent) are mixed, and the mixture is kneaded and dispersed using a disperser to prepare an ink containing a high concentration of silica particles (concentration of silica particles: 35% by mass).

[0185] Next, a predetermined amount of the ink was added to 100 parts by mass of the polyester polyol resin solution and 64.4 parts by mass of ethyl acetate, and mixed and dispersed using a disperser to prepare a main agent of an external adhesive containing silica particles.

[0186] With respect to 100 parts by mass of the main agent, 7.1 parts by mass of an adduct of toluene diisocyanate (TDI) (aromatic system) and trimethylolpropane (NCO is 13.0% by mass, solid content is 75% by mass) as an aromatic isocyanate compound was added as a curing agent, and 34.1 parts by mass of ethyl acetate was further added, and stirred and mixed to prepare an outer adhesive composition containing silica particles (i.e., a two-component curable polyester urethane resin containing silica particles). In the outer adhesive composition, the molar ratio (-NCO) / (-OH) of the isocyanate functional group (-NCO) to the polyester polyol hydroxyl group (-OH) was 10, and the content of the silica particles in the outer adhesive composition was 2.2% by mass.

[0187] Next, a cured film of the outer adhesive composition was prepared by the following method, and its physical properties were evaluated.

[0188] That is, the outer adhesive composition is applied in a layer on a non-adhesive untreated polypropylene film so that the thickness after drying is 10 μm, the solvent in the composition is dried and evaporated, and then the composition is aged at 60° C. until the residual isocyanate is 5% by mass or less, thereby curing. Then, the cured product is peeled off from the untreated polypropylene film, thereby preparing a cured film (10 μm thick) of the outer adhesive composition.

[0189] The cured film was cut into a 15 mm width to obtain a test piece, and then the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation L. As a result, the tensile breaking strength was 31 MPa and the tensile breaking elongation L was 23%.

[0190] Therefore, the improvement rate ΔL (={(L-L0) / L0}×100%) of the tensile elongation at break of the cured film of the external adhesive composition due to the inclusion of the silica particles was 28%.

[0191] Next, at 9.5 g / m2 The outer adhesive composition is applied in a layer on the outer surface of the aluminum foil with a coating amount (specifically, the solid content coating amount. The same applies below), and the solvent in the composition is dried and evaporated. Then, the outer surface of the aluminum foil is bonded to the inner surface of the biaxially stretched nylon film (heat-resistant resin layer 3) and aged at 60°C to cure the composition. In this case, the content of silica particles in the outer adhesive layer 5R is 0.21 g / m 2 .

[0192] Next, an acid-modified polypropylene (PP) adhesive was prepared as an inner adhesive composition constituting the inner adhesive. The method for preparing the composition is as follows.

[0193] That is, 0.9 parts by mass of a polymer (polyfunctional isocyanate compound) of hexamethylene diisocyanate (HDI) as a curing agent was added to 15 parts by mass of an acid-modified polypropylene resin solution and 85 parts by mass of a mixed organic solvent of methylcyclohexane:methyl ethyl ketone=8 parts by mass:2 parts by mass so that the equivalent ratio (NCO / OH) became 1.8, and the mixture was stirred and mixed to prepare the above-mentioned inner adhesive composition.

[0194] Next, a cured film of the inner adhesive composition was prepared by the following method, and its physical properties were evaluated.

[0195] That is, the inner adhesive composition is applied in a layer on a non-adhesive untreated polypropylene film so that the thickness after drying is 10 μm, the solvent in the composition is dried and evaporated, and then the composition is aged at 40° C. until the residual isocyanate is 5% by mass or less, thereby curing. Then, the cured product is peeled off from the untreated polypropylene film, thereby preparing a cured film (10 μm thick) of the inner adhesive composition.

[0196] The cured film was cut into 15 mm width to collect a test piece, and then the test piece was subjected to a tensile test to measure the tensile breaking strength and tensile breaking elongation. As a result, the tensile breaking strength was 20 MPa and the tensile breaking elongation was 105%.

[0197] Next, at 5.5 g / m 2 The inner surface of the aluminum foil is coated with the above-mentioned inner adhesive composition in a layered manner with a coating amount (specifically, the solid content coating amount. The same below) to dry and evaporate the solvent in the composition. Then, the inner surface of the aluminum foil is bonded to the outer surface of the above-mentioned unstretched three-layer co-extruded polypropylene (CPP) film as the thermally fusible resin layer 4, and aged at 40°C to cure the composition.

[0198] The packaging material was manufactured by the above method.

[0199] <Example 2>

[0200] In Example 1, the insulating agent is silicon dioxide particles (SiO2 particles: number average particle size of 0.03 μm, specific surface area of ​​150 m 2 / g, volume resistivity is 1×10 16 Ωcm) and the content of the silica particles in the outer adhesive composition was 5.0 mass %, and the coating amount of the outer adhesive composition was 5.0 g / m 2 , except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of the outer adhesive composition and to produce a packaging material. In this case, the content of the silica particles in the outer adhesive layer 5R was 0.25 g / m 2 .

[0201] The tensile elongation at break and its increase rate ΔL values ​​of the cured film of the outer adhesive composition measured and calculated by the tensile test are recorded in the "Cured Film" column of "Outer Adhesive Layer" in Table 1. The same applies to Examples 3 to 10 and Comparative Examples 1 and 2.

[0202] <Example 3>

[0203] In Example 1, the insulating agent is silicon dioxide particles (SiO2 particles: number average particle size of 0.01 μm, specific surface area of ​​330 m 2 / g, volume resistivity is 1×10 16 Ωcm) and the content of the silica particles in the outer adhesive composition was 9.5 mass %, and the coating amount of the outer adhesive composition was 8.5 g / m 2 , except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of the outer adhesive composition and to produce a packaging material. In this case, the content of the silica particles in the outer adhesive layer 5R was 0.81 g / m 2 .

[0204] <Example 4>

[0205] In Example 1, the insulating agent is silicon dioxide particles (SiO2 particles: number average particle size of 0.4 μm, specific surface area of ​​10 m 2 / g, volume resistivity is 1×10 16 Ωcm) and the content of silica particles in the outer adhesive composition was 1.3 mass %, and the coating amount of the outer adhesive composition was 8.0 g / m 2, except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of the outer adhesive composition and to produce a packaging material. In this case, the content of the silica particles in the outer adhesive layer 5R was 0.10 g / m 2 .

[0206] <Example 5>

[0207] In Example 1, the insulating agent is made of silica particles (SiO2 particles: number average particle size of 4.0 μm, specific surface area of ​​1.0 m 2 / g, volume resistivity is 1×10 16 Ωcm) and the content of the silica particles in the outer adhesive composition was 3.3 mass %, and the coating amount of the outer adhesive composition was 6.0 g / m 2 , except for this, the same operation as in Example 1 was performed to conduct a tensile test of the cured film of each adhesive composition and to produce a packaging material. In this case, the content of the silica particles in the outer adhesive layer 5R was 0.20 g / m 2 .

[0208] <Example 6>

[0209] In Example 1, the outer adhesive is acrylic polyol (which is a type of acrylic adhesive (main agent)), the curing agent is a polymer of hexamethylene diisocyanate (HDI), and the insulation reinforcing agent is calcium carbonate particles (CaCO3 particles: number average particle size of 0.03 μm, specific surface area of ​​130 m 2 / g, volume resistivity is 1×10 14 Ωcm) and the content of calcium carbonate particles in the outer adhesive composition was 9.0 mass %, and the coating amount of the outer adhesive composition was 8.0 g / m 2 , except for this, the tensile test of the cured film of the outer adhesive composition was carried out in the same manner as in Example 1, and the outer surface of the aluminum foil was bonded to the inner surface of the biaxially stretched nylon film (heat-resistant resin layer 3), and the composition was cured by aging at 60°C. In this case, the content of calcium carbonate particles in the outer adhesive layer 5R was 0.72 g / m 2 .

[0210] Next, a carboxylic acid-modified polypropylene resin is used as an inner adhesive resin. While the melted inner adhesive resin is flowed between the inner surface of the aluminum foil and the unstretched three-layer co-extruded polypropylene film (thermo-fusible resin layer 4), the aluminum foil and the unstretched three-layer co-extruded polypropylene film are laminated together by a sandwich lamination method, and the inner adhesive resin is aged at 40°C.

[0211] The packaging material was manufactured by the above method.

[0212] <Example 7>

[0213] In Example 6, the content of calcium carbonate particles in the outer adhesive composition was set to 3.0 mass % and the coating amount of the outer adhesive composition was set to 6.5 g / m 2 , except for this, the same operation as in Example 6 was performed to conduct a tensile test of the cured film of the outer adhesive composition and to produce a packaging material. In this case, the content of calcium carbonate particles in the outer adhesive layer 5R was 0.20 g / m 2 .

[0214] <Example 8>

[0215] In Example 6, the insulation enhancing agent is calcium carbonate particles (CaCO3 particles: number average particle size of 3.0 μm, specific surface area of ​​0.8 m 2 / g, volume resistivity is 1×10 14 Ωcm) and the content of calcium carbonate particles in the outer adhesive composition was 3.3 mass %, and the coating amount of the outer adhesive composition was 6.0 g / m 2 , except for this, the same operation as in Example 6 was performed to conduct a tensile test of the cured film of the outer adhesive composition and to produce a packaging material. In this case, the content of calcium carbonate particles in the outer adhesive layer 5R was 0.20 g / m 2 .

[0216] <Example 9>

[0217] In Example 6, the insulating agent is silicon dioxide particles (SiO2 particles: number average particle size of 0.2 μm, specific surface area of ​​25 m 2 / g, volume resistivity is 1×10 16 Ωcm) and the content of the silica particles in the outer adhesive composition was 8.5 mass %, and the coating amount of the outer adhesive composition was 3.0 g / m 2 , except for this, the same operation as in Example 6 was performed to conduct a tensile test of the cured film of the outer adhesive composition and to produce a packaging material. In this case, the content of the silica particles in the outer adhesive layer 5R was 0.26 g / m 2 .

[0218] <Example 10>

[0219] In Example 6, the insulating reinforcing agent is acrylic resin particles (with a number average particle size of 2.0 μm and a specific surface area of ​​2.5 m 2 / g, volume resistivity is 1×10 15Ωcm), and the content rate of the acrylic resin particles in the outer adhesive composition was 5.5 mass%, and the coating amount of the outer adhesive composition was 4.5 g / m 2 , other than that, the operation was the same as in Example 6, a tensile test of the cured film of the outer adhesive composition was performed, and a packaging material was manufactured. In this case, the content of the acrylic resin particles in the outer adhesive layer 5R was 0.25 g / m 2 .

[0220] <Comparative Example 1>

[0221] In Example 1, the outer adhesive layer did not contain an insulating property enhancer, and the coating amount of the outer adhesive composition was 5.0 g / m 2 , other than that, the operation was the same as in Example 1, and a packaging material was manufactured.

[0222] <Comparative Example 2>

[0223] In Example 6, the outer adhesive layer did not contain an insulating property enhancer, and the coating amount of the outer adhesive composition was 5.0 g / m 2 , other than that, the operation was the same as in Example 6, and a packaging material was manufactured.

[0224] (Method for measuring specific surface area)

[0225] In the above Examples 1 to 10 and the above Comparative Examples 1 to 2, the specific surface area of the insulating property enhancer (insulating property enhancing particles) was measured by the following method in accordance with JIS Z8330:2013.

[0226] That is, the enhancer was weighed, and using a gas adsorption type pore size distribution analyzer (NOVA4200e: Seishin Enterprise Co., Ltd.), after pretreatment of the weighed enhancer by the N2 gas purge method (gas flow rate was 20 cm 3 / min, gas pressure was 20 kPa, heating temperature was 200 °C, treatment time was 2 hours), the specific surface area of the insulating property enhancer was measured by the BET multi-point method.

[0227] (Method for measuring volume resistivity)

[0228] In the above Examples 1 to 10 and the above Comparative Examples 1 to 2, as Figure 4 shown, using an insulation resistance meter 59 and an electrode with a guard (Japanese: “ガード付き電極”), in accordance with ASTM D257, the volume resistivity of the insulating property enhancer (insulating property enhancing particles) 60 was measured according to the following steps 1 to 6.

[0229] It should be noted that the electrode 50 with a protective cover includes a main electrode 51 (diameter of 25 mm), a protective electrode 52, and a counter electrode 53 (size of 50 mm×50 mm), and the gap d between the two electrodes 51 and 53 is 10 mm. In addition, as the insulation resistance meter 59, a digital ultra-high resistance / micro-current meter "5450" manufactured by ADC Co., Ltd. (Japanese: "ADC Co., Ltd.") is used. In this figure, in order to make the structure of the electrode 50 with a protective cover easier to understand, the main electrode 51, the protective electrode 52, and the counter electrode 53 are marked with cross hatching, and the insulation enhancer 60 is marked with dot hatching.

[0230] Step 1: In the filling portion of the electrode 50 with a protective cover, the insulating reinforcing agent 60 is fully charged into the measuring container 57 .

[0231] Step 2: The measuring container 57 is lifted to a height of 10 cm and then dropped, thereby compressing and filling the measuring container 57 with the insulating reinforcing agent 60 .

[0232] Step 3: After repeating the lifting-dropping operation 50 times, the lead wires 55 , 55 extending from the main electrode 51 and the counter electrode 53 are connected to the insulation resistance meter 59 .

[0233] Step 4: Turn on the application switch of the insulation resistance meter 59, and read the resistance value after 1 minute of power-on time under the condition of an applied voltage of 500V.

[0234] Step 5: Take out the electrode 50 with the protective cover, weigh the insulation reinforcing agent 60 sandwiched between the two electrodes 51 and 53, and calculate the packing density of the insulation reinforcing agent 60.

[0235] Step 6: Use the effective area of ​​the main electrode 51 (491mm 2 ), the gap d (10 mm) between the two electrodes 51 and 53, the applied voltage (500 V), the resistance value and the filling density of the insulating reinforcing agent 60, and calculate the volume resistivity of the insulating reinforcing agent 60.

[0236] (Method for calculating number average particle size)

[0237] The number average particle size of the insulation-reinforcing particles is determined by the following method.

[0238] A suspension of insulation-enhancing particles was prepared, and the particle size distribution of the insulation-enhancing particles was measured using a laser diffraction / scattering particle size distribution analyzer (Partica LA-960V2: Horiba, Ltd.) to determine the number average particle size of the insulation-enhancing particles.

[0239] (Evaluation of packaging materials)

[0240] The packaging materials of Examples 1 to 10 and Comparative Examples 1 to 2 were subjected to puncture strength measurement and moldability test. The results are shown in Table 1 below.

[0241] [Table 1]

[0242]

[0243] <Punch Strength>

[0244] The puncture strength of the packaging material is measured in accordance with JIS Z1707: 2019. The puncture strength test at this time is performed according to the following steps 1 and 2.

[0245] Step 1: Fix the test piece collected from the packaging material with a fixture, and pierce a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm from the heat-resistant resin layer side at a test speed of 50±5 mm / min, and measure the maximum force (N) until the needle penetrates.

[0246] Step 2: The number of test pieces collected from the packaging material is set to 5 or more, and the test pieces are collected so as to be averaged over the entire width of the packaging material.

[0247] The meanings of the symbols in the "Piercing Strength" column in Tables 1 and 2 are as follows: ◎ and ○ were regarded as passing the piercing strength test.

[0248] ◎: Puncture strength greater than 19N

[0249] ○: Puncture strength greater than 16N and less than 19N

[0250] ×: The puncture strength is 16N or less.

[0251] <Molding processability test>

[0252] A press machine manufactured by AMAD A Co., Ltd. was prepared, which was provided with a die having a punch shape of 33 mm×54 mm, a punch corner R of 2 mm, a punch shoulder R of 1.3 mm, and a die shape of a die shoulder R of 1 mm.

[0253] Then, a rectangular test plate of 100 mm in length and 125 mm in width was collected from the packaging material, and the test plate was deep-drawn using the above-mentioned press machine to form a formed product.

[0254] In a dark room, the presence of pinholes and cracks (cracks) in the corners of the molded product is confirmed by the transmitted light method, and the "maximum molding depth (mm)" without pinholes and cracks is investigated to evaluate the molding processability of the packaging material. The evaluation criteria are as follows. It should be noted that ◎ and ○ are considered to be qualified in the molding processability test.

[0255] ◎: No cracks or pinholes when the maximum forming depth is 7mm or more

[0256] ○: No cracks or pinholes when the maximum forming depth is 6 mm or more and less than 7 mm

[0257] ×: There are cracks and / or pinholes when the maximum forming depth is less than 6 mm.

[0258] As is apparent from Table 1, it was confirmed that the packaging materials of Examples 1 to 10 containing an insulation reinforcing agent in the outer adhesive layer had high puncture strength.

[0259] Furthermore, it was confirmed that, as in Examples 1 to 3, 6, 7, 9 and 10, the number average particle size of the insulation-enhancing particles was in the range of 0.01 μm to 3 μm, and the specific surface area of ​​the insulation-enhancing particles was 1 m 2 / g or more and the content of the insulating reinforcing agent in the outer adhesive layer 5R is 0.2g / m 2 ~1.0g / m 2 When it is within the range of , the improvement rate ΔL of the tensile elongation at break is very large, so the molding processability of the packaging material is high.

[0260] This application claims priority to Japanese Patent Application No. 2022-169760 filed on October 24, 2022 and Japanese Patent Application No. 2023-145340 filed on September 7, 2023, the disclosures of which directly constitute a part of this application.

[0261] The terms and expressions used herein are for explanation and are not intended to be interpreted in a limiting sense. Any equivalents of the features shown and described herein are not excluded. It should be understood that various modifications are allowed within the scope of the claims of the present utility model.

[0262] Industrial Applicability

[0263] The utility model can be used in packaging materials, packaging shells and power storage devices for molding processing.

Claims

1. A packaging material for molding, comprising a metal foil layer, a heat-resistant resin layer disposed on the outer surface side of the metal foil layer, and a heat-fusible resin layer disposed on the inner surface side of the metal foil layer, characterized in that: An outer adhesive layer is provided between the metal foil layer and the heat-resistant resin layer, and an inner adhesive layer is provided between the metal foil layer and the heat-fusible resin layer. The outer adhesive layer contains an insulation reinforcing agent.

2. The packaging material for molding processing according to claim 1, wherein As the insulation enhancing agent, insulation enhancing particles are used, and The number average particle size of the insulation-enhancing particles is in the range of 0.01 μm to 3 μm.

3. The packaging material for molding processing according to claim 1 or 2, wherein: As the insulation enhancing agent, insulation enhancing particles are used, and The specific surface area of ​​the insulation enhancing particles is 1 m 2 / g or above.

4. The packaging material for molding processing according to claim 1 or 2, wherein: As the insulation enhancing agent, insulation enhancing particles are used, and The volume resistivity of the insulating enhanced particles is 1×10 12 Ωcm or more.

5. The packaging material for molding processing according to claim 1 or 2, wherein: The outer adhesive layer is formed of a cured film of an outer adhesive composition containing an outer adhesive and the insulation reinforcing agent. The tensile elongation at break of the cured film of the outer adhesive composition is defined as L. When the tensile elongation at break of a cured film of an external adhesive composition containing the external adhesive but not containing the insulation reinforcing agent is defined as L0, The L satisfies the following relation 1, 15%≤{(L-L0) / L0}×100%≤250%…(Formula 1).

6. The packaging material for molding processing according to claim 1 or 2, wherein: The outer adhesive layer is 2g / m 2 ~10g / m 2 A coating amount in a range of is provided between the metal foil layer and the heat-resistant resin layer, The content of the insulating reinforcing agent in the outer adhesive layer is 0.2 g / m 2 ~1.0g / m 2 within the range.

7. A packaging shell, characterized in that: The packaging case is formed by deep drawing or stretching the packaging material for molding according to any one of claims 1 to 6.

8. An electric storage device comprising an electric storage device body and a packaging case packaging the electric storage device body, characterized in that: As the packaging case, the packaging case according to claim 7 is provided.