MOF-containing aramid fiber aerogel as well as preparation method and application thereof

By pretreating aramid nanofibers to grow MOF in situ, MOF-loaded aerogels with high loading capacity and high specific surface area are prepared, which solves the problems of CO2 adsorption and processing performance of MOF fabrics and achieves efficient adsorption and stability.

CN118772647AInactive Publication Date: 2024-10-15TIANJIN POLYTECHNIC UNIV
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202310358562.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing MOF fabrics have problems with porosity and insufficient utilization of active sites in terms of carbon dioxide adsorption, and their processing performance is poor, making it difficult to improve their detoxification performance.

Method used

By pretreatment of aramid nanofibers, MOF can be grown in situ and loaded, and MOF-loaded aramid nanofiber aerogels can be prepared to increase the MOF loading capacity and specific surface area and maintain mechanical properties and thermal insulation properties.

Benefits of technology

It achieves efficient carbon dioxide adsorption, good structural stability and flame retardant properties, and does not require complex pretreatment to maintain the protective properties of the fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772647A_ABST
    Figure CN118772647A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of carbon dioxide adsorption, in particular to MOF-containing aramid fiber aerogel as well as a preparation method and application thereof. The aramid fiber aerogel containing the MOF is prepared from the MOF and aramid fiber nanofibers; the loading capacity of the MOF is 60 to 270 percent; wherein, the MOF is UiO-66-NH2; the thermal conductivity coefficient of the MOF-loaded aramid nanofiber aerogel is smaller than 30 mW / mk, the specific surface area is 280-590 m < 2 > / g, the pore volume is 0.25-0.35 cm < 3 > / g, and the average pore size is 1.4-1.6 nm. The ANF is pretreated by the ATA, so that the ATA is attached to the surface of the fiber, and a nucleation site is provided for subsequent growth of the MOF. The MOF-loaded aramid nanofiber aerogel prepared by the method disclosed by the invention is high in MOF loading capacity, high in carbon dioxide adsorption efficiency and good in structural stability, flame retardance, heat insulation and compression performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon dioxide adsorption, and in particular to an aramid nanofiber aerogel carrying MOF, and a preparation method and application thereof. Background Art

[0002] The sharp increase in anthropogenic CO2 concentration will trigger a serious greenhouse effect, which will lead to severe global warming and related natural disasters, glacier melting and extreme climate. The development and application of carbon dioxide capture and utilization technology (CCU) plays an important role in mitigating global warming and has therefore received great attention. In recent years, metal-organic frameworks (MOFs) composed of organic ligands and inorganic metal centers have shown significant advantages in the degradation and adsorption of CWAs due to their unique structure and abundant active sites. Among them, Zr6-based MOFs such as MOF-808, UiO-66-NH2, and UMCM-313 have attracted much attention due to their efficient catalytic hydrolysis of CWAs at room temperature. In order to overcome the defects of poor processing performance and difficult handling of MOF powders, synthetic polymers are usually fixed on cotton, silk and nanofibers by physical spraying, layer-by-layer self-assembly, co-electrospinning and direct growth of MOFs on fibers. However, these MOF fabrics inevitably face the challenges of complex pretreatment to improve the affinity of MOF to fibers (complex pretreatment will reduce the mechanical properties, thermal insulation and other protective properties of the fabric), as well as reduced accessibility of pores blocked by binders, which has a great impact on their detoxification performance. In addition, in actual environments, they are often accompanied by multiple threats such as combustion and high temperature. Therefore, CO2 adsorption materials with high porosity and active sites are very necessary, but still challenging. Summary of the invention

[0003] Based on the above content, the present invention provides an aramid aerogel containing MOF and a preparation method and application thereof. By pretreating aramid nanofibers (ANF), MOF is loaded onto ANF through in-situ growth. The prepared MOF-loaded aramid nanofiber aerogel has the advantages of high MOF loading and large specific surface area.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] One of the technical solutions of the present invention is an aramid aerogel containing MOF, wherein the aramid nanofiber aerogel containing MOF comprises MOF and aramid nanofibers; the loading amount of the MOF is 60-270%; the MOF is UiO-66-NH2; the thermal conductivity of the aramid nanofiber aerogel loaded with MOF is less than 30mW / mk, and the specific surface area is 280-590m 2 / g, pore volume is 0.25-0.35cm 3 / g, and the average pore size is 1.4-1.6nm.

[0006] The second technical solution of the present invention is a method for preparing the above-mentioned MOF-containing aramid aerogel, comprising the following steps:

[0007] Step 1, placing aramid nanofibers in N,N-dimethylformamide to prepare an ANF / DMF dispersion, then adding 2-aminoterephthalic acid and stirring to obtain a pre-reaction solution;

[0008] Step 2, adding MOF precursor and glacial acetic acid to the pre-reaction solution and mixing them evenly to obtain a reaction solution;

[0009] Step 3, subjecting the reaction solution to a solvothermal reaction, followed by washing and replacing the solvent to obtain an aramid nanofiber solution loaded with MOF;

[0010] Step 4, adding tert-butyl alcohol, water and blocked isocyanate (B-MDI) to the MOF-containing aramid nanofiber solution to prepare a dispersion, followed by freeze-drying and activation to obtain the MOF-loaded aramid nanofiber aerogel.

[0011] Furthermore, in step 1, the concentration of the ANF / DMF dispersion is 0.4wt%; and the mass ratio of the aramid nanofiber to the 2-aminoterephthalic acid is 1:1.

[0012] Furthermore, in step 2, the MOF precursor is a mixture of zirconium salt and 2-aminoterephthalic acid in a molar ratio of 1:1; the mass ratio of the MOF precursor to the aramid nanofiber is 0.3-2:1; the molar ratio of the glacial acetic acid to the zirconium salt is 200:1; the stirring is specifically: stirring at room temperature for 0.5-4h; and the zirconium salt is zirconium chloride.

[0013] Furthermore, in step 3, the solvent thermal reaction is specifically: reacting at 120° C. for 12 hours; washing with DMF and methanol; and replacing the solvent with water.

[0014] Furthermore, in step 4, the mass ratio of tert-butyl alcohol to water is 1:10; the amount of blocked isocyanate added is 0.1% of the content of aramid nanofibers; and the concentration of MOF-loaded aramid nanofibers in the dispersion is 0.15-0.25wt%.

[0015] The blocked isocyanate (B-MDI) has no effect on the loading amount of MOF in the aerogel, and its role in the present invention is to improve the compression performance of the prepared aerogel.

[0016] Furthermore, the preparation method of the blocked isocyanate (B-MDI) comprises the following steps:

[0017] 30g of n-butanol solution was added to 70g of N,N-dimethylacetamide to prepare a 30wt% n-butanol solution, and 50g of 4,4-diphenylmethane diisocyanate was added under a constant temperature water bath at 40°C. Then, under nitrogen protection, 98.67g of n-butanol solution was added dropwise to the mixed solution in the reactor, and magnetic stirring was performed. After reacting for 2h, the solution was placed in a vacuum oven at 40°C and vacuum dried to obtain B-MDI.

[0018] Furthermore, in step 4, the freeze-drying step also includes a freeze-molding step.

[0019] Furthermore, in step 4, the activation is specifically performed under vacuum conditions at 80° C. for 12 hours.

[0020] The third technical solution of the present invention is the use of the above-mentioned MOF-loaded aramid nanofiber aerogel in the preparation of chemical warfare agent protection materials.

[0021] The present invention discloses the following technical effects:

[0022] The present invention does not require complicated pretreatment such as heating and metallization of ANF, and will not affect the mechanical properties, thermal insulation properties and other protective properties of ANF; the present invention pretreats ANF with ATA so that ATA adheres to the fiber surface, providing nucleation sites for the subsequent growth of MOF. The MOF-loaded aramid nanofiber aerogel prepared by the method of the present invention has a high MOF loading amount, high carbon dioxide adsorption efficiency, and good structural stability, flame retardancy, thermal insulation and compression properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 The figures are the actual pictures of the ANF / DMF dispersion (a) and the ATA@ANF / DMF dispersion (b) of the present invention.

[0025] Figure 2 Infrared images of ANF and ATA@ANF aerogels of the present invention.

[0026] Figure 3 These are SEM images of the UiO-66-NH2@ANF aerogel at different magnifications (a), TEM images of the UiO-66-NH2@ANF aerogel and Mapping images (b).

[0027] Figure 4Actual pictures of the ANF aerogel (a) and UiO-66-NH2@ANF aerogel (b) of the present invention.

[0028] Figure 5 These are SEM images of the UiO-66-NH2@ANF aerogel of the present invention; among them, (a) UiO-66-NH2@ANF-0.3 aerogel, (b) UiO-66-NH2@ANF-0.5 aerogel, (c) UiO-66-NH2@ANF-1 aerogel, and (d) UiO-66-NH2@ANF-2 aerogel.

[0029] Figure 6 Schematic diagram of the loading capacity of several UiO-66-NH2@ANF aerogels of the present invention.

[0030] Figure 7 This is the infrared curve of the UiO-66-NH2@ANF aerogel of the present invention.

[0031] Figure 8 TG curves (a) of UiO-66-NH2 and UiO-66-NH2@ANFA-X of the present invention, and XRD curves (b) of ANF, UiO-66-NH2 and UiO-66-NH2@ANFA-X.

[0032] Fig. 9 (a) N2 adsorption-desorption curve and (b) pore size distribution diagram of UiO-66-NH2@ANF aerogel of the present invention.

[0033] Fig.10 GC curves of CEES degradation by UiO-66-NH2@ANF aerogel of the present invention; wherein (a) UiO-66-NH2@ANF-2 aerogel, (b) UiO-66-NH2@ANF-2 aerogel and (c) UiO-66-NH2@ANF-2 aerogel.

[0034] Fig.11 The degradation rate (a) and half-life (b) of the aerogel of the present invention on CEES.

[0035] Fig.12 GC-MS analysis of CEES degradation by UiO-66-NH2@ANF-1 aerogel of the present invention (a) and mechanism diagram of CEES degradation by UiO-66-NH2@ANF-1 aerogel (b, c).

[0036] Fig.13The degradation rate of the UiO-66-NH2@ANF-1 aerogel of the present invention after repeated use for three times (a), the infrared (b) and XRD (c) of the UiO-66-NH2@ANF-1 aerogel after repeated use for three times, and the SEM image of the UiO-66-NH2@ANF-1 aerogel after the third degradation (d).

[0037] Fig.14 The height of UiO-66-NH2@ANF aerogel of the present invention (a), infrared thermal images (b), temperature change curve within 30 minutes (c), and thermal conductivity (d) of UiO-66-NH2@ANF aerogels with concentrations of 0.15wt%, 0.20wt%, and 0.25wt%.

[0038] Fig.15 The stress-strain curves of the UiO-66-NH2@ANF-1 aerogel of the present invention at 10%, 30%, 50% and 70% respectively (a), the stress-strain curve of the UiO-66-NH2@ANF-1 aerogel cycled 100 times under 30% constant compression (b), the compression-rebound process and the optical image of the UiO-66-NH2@ANF-1 aerogel after 100 compressions (c).

[0039] Fig.16 It is the moisture diffusion position of the UiO-66-NH2@ANF-1 aerogel of the present invention. DETAILED DESCRIPTION

[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0041] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0045] Unless otherwise specified, the chemical reagents and equipment used in the embodiments of the present invention can be obtained through commercial channels.

[0046] The aramid nanofibers used in the embodiments of the present invention are prepared by the following steps:

[0047] The sodium hydroxide is dissolved in distilled water to prepare a 15wt% alkaline solution; aramid staple fibers (AMFs) are chopped; the chopped aramid staple fibers are added to the prepared alkaline solution at a bath ratio of 1:250, stirred at 80°C for 4 hours, then filtered, washed with water to neutrality, and finally adjusted to a 0.4wt% solution. After 30 cycles of treatment with a nanocellulose instrument, a uniformly dispersed aramid nanofiber aqueous dispersion is obtained, and then the aramid nanofiber aqueous dispersion is filtered and replaced with DMF dispersion with N,N-dimethylformamide, and the concentration is 0.4wt%, namely, aramid nanofiber dispersion (ANF / DMF dispersion).

[0048] The aramid nanofiber dispersion obtained through other channels, such as purchase, is also applicable to the present invention.

[0049] The B-MDI used in the embodiment of the present invention is prepared by the following steps:

[0050] 30g of n-butanol solution was added to 70g of N,N-dimethylacetamide to prepare a 30wt% n-butanol solution, and 50g of 4,4-diphenylmethane diisocyanate was added under a constant temperature water bath at 40°C. Then, under nitrogen protection, 98.67g of n-butanol solution was added dropwise to the mixed solution in the reactor, and magnetic stirring was performed. After 2h, the solution was placed in a vacuum oven at 40°C and vacuum dried to obtain B-MDI.

[0051] The "room temperature" and "normal temperature" mentioned in the present invention, unless otherwise specified, all mean 20-30°C.

[0052] Example 1

[0053] Pretreatment of aramid nanofibers: A certain amount of 2-aminoterephthalic acid (ATA, the mass ratio of ATA to aramid nanofibers is 1:1) was added to the aramid nanofiber dispersion and stirred at room temperature for a certain period of time to obtain a pre-reaction solution (ATA@ANF / DMF dispersion).

[0054] This example explores the effects of two variables on the loading of UiO-66-NH2 (MOF). First, pretreatment at different times: stirring for different times after adding ATA, i.e., adding MOF precursor (MOF precursor is zirconium chloride and ATA, zirconium chloride and ATA molar ratio is 1:1; MOF precursor addition amount is: MOF precursor: ANF mass ratio is 1:1) and glacial acetic acid (glacial acetic acid: zirconium chloride molar ratio = 200:1) after 0h, 0.5h and 4h, and stirring thoroughly; second, under the premise of pretreatment for 4 hours, adding 2 times, 1 times, 0.5 times and 0.3 times the fiber mass of MOF precursor (MOF precursor is zirconium chloride and ATA, zirconium chloride: ATA molar ratio = 1:1), adding glacial acetic acid (glacial acetic acid: zirconium chloride molar ratio = 200:1), stirring thoroughly.

[0055] Solvothermal reaction: After the above solutions are stirred evenly, they are poured into the reaction kettle respectively and reacted at 120°C for 12 hours.

[0056] Washing and replacement: The solution poured out from the reactor was washed three times with DMF and methanol respectively to remove the acid and unreacted ligand, and then the solvent was replaced with distilled water.

[0057] Preparation of solution: Add tert-butyl alcohol (TBA) and distilled water (TBA: H2O mass ratio = 1:10) and B-MDI (B-MDI amount is 0.1% of ANF content) to the solution after the above solvent replacement to prepare 0.15wt%, 0.2wt%, and 0.25wt% dispersions.

[0058] Freezing molding: Pour the above dispersion into the prepared molds respectively and freeze them in a refrigerator.

[0059] Freeze drying: The frozen dispersion was placed in a freeze dryer to remove the solvent to obtain UiO-66-NH2@ANF aerogel. The aerogels obtained with different pretreatment times were recorded as UiO-66-NH2@ANF-0h aerogel, UiO-66-NH2@ANF-0.5h aerogel, and UiO-66-NH2@ANF-4h aerogel; the aerogels obtained with different MOF precursor addition amounts were recorded as UiO-66-NH2@ANF-2 aerogel, UiO-66-NH2@ANF-1 aerogel, UiO-66-NH2@ANF-0.5 aerogel, and UiO-66-NH2@ANF-0.3 aerogel.

[0060] Vacuum activation: The several aerogels obtained above were activated in a vacuum oven at 80°C for 12 hours to remove impurities in the MOF molecules.

[0061] The following tests were performed on the aerogel prepared in Example 1:

[0062] 1. Structural characterization

[0063] 1.1 Determination of aerogel density

[0064] The mass of the aerogel was weighed on a balance and recorded as m (in g). The height h (in cm) and diameter d (in cm) of the aerogel were measured with a ruler. The density of the aerogel was calculated according to the density formula (ρ = m / v), where:

[0065] 1.2 Calculation of UiO-66-NH2 loading on ANF

[0066] The loading amount was calculated according to the following formula, where l is the loading amount; w0 is the dry weight of the fiber before the solvothermal reaction, in g; and w1 is the total dry weight of the fiber plus MOF after the solvothermal reaction, in g.

[0067]

[0068] 1.3 Fourier infrared spectroscopy test

[0069] The functional groups of aramid nanofiber aerogel, UiO-66-NH2, and UiO-66-NH2@ANF aerogel were analyzed and characterized by Fourier transform infrared spectrometer, and the changes of the groups before and after ANF loading UiO-66-NH2 were compared. The scanning range of the test was 4000~400cm -1 .

[0070] 1.4 X-ray electron spectrum test

[0071] X-ray photoelectron spectroscopy (XPS) was used to characterize the changes in the surface chemical composition and group composition of aramid nanofiber aerogel and ATA@ANF aerogel samples to verify the promoting effect of ATA pretreatment on the loading of UiO-66-NH2.

[0072] 1.5 Thermal field emission scanning electron microscopy observation

[0073] The aerogel sample was glued to an aluminum sheet with conductive glue, sprayed with gold and dried overnight, and then the growth of MOF along the fiber was observed under a thermal field emission scanning electron microscope.

[0074] 1.6 X-ray diffraction test

[0075] The crystal structure of aramid nanofiber aerogel, UiO-66-NH2, and UiO-66-NH2@ANF aerogel was analyzed by X-ray diffractometer (D8 ADVANCE). The working current was 40 mA, the working voltage was 40 kV, the 2θ was 5-50°, and the scanning speed was 8° min -1 .

[0076] 1.7 Specific surface area and porosity analysis

[0077] The specific surface area, average pore size, adsorption-desorption curve, pore size distribution curve, etc. of the sample can be obtained by the fully automatic specific surface area and porosity analyzer (Autosorb-iQ) to verify the catalytic activity of the sample. Before the test, the sample was degassed at 200°C in a N2 atmosphere for 3 h, and then a N2 adsorption test was performed at 70K.

[0078] 1.8 Comprehensive thermal analysis

[0079] The UiO-66-NH2 loading on different samples can be roughly compared by using a comprehensive thermal analyzer (STA 449F5). The gas atmosphere during the test was nitrogen, the temperature range was from room temperature to 1000°C, and the heating rate was 10°C / min.

[0080] 2. CEES (mustard gas simulant) degradation

[0081] First, the brown rubber stoppered vial used as the reaction container was dried at 70 °C for 12 hours to remove physically adsorbed water. 20 mg of UiO-66-NH2@ANF aerogel was placed in the drying container and covered with a rubber stopper. In the fume hood, 5 μl of CEES was injected into the vial using a microinjector. Then, the container was placed in a closed and dark constant temperature oscillator for different reaction times of 10 min to 72 h. Subsequently, 2 ml of acetonitrile was added to the above reaction container using a syringe needle, and the product was extracted after 30 min of extraction on a shaker. The reaction progress was monitored by gas chromatography (Agilent 7890B), and finally, the degradation products were detected by gas chromatography-mass spectrometry (TRACE1300-ISQ7000).

[0082] 3. Thermal protection performance test

[0083] 3.1 Thermal insulation performance test

[0084] Thermal insulation is an important parameter to characterize thermal protection performance. Thermal insulation performance can be expressed by thermal conductivity. The smaller the thermal conductivity, the better the thermal insulation performance of the sample. The present invention adopts the transient plane heat source method and uses a thermal conductivity tester to test the sample in accordance with ISO 22007-2008 standard. Each aerogel sample is tested 5 times at room temperature. Aerogel samples of different concentrations are placed on a heating table at 200°C, and the changes in the surface temperature of the aerogel over time are recorded by an infrared thermal imager.

[0085] 3.2 Flame retardant performance test

[0086] Flame retardant properties are characterized by the Limiting Oxygen Index (LOI). Generally speaking, LOI < 22 is a flammable material, LOI between 22 and 27 is a combustible material, and LOI > 27 is a flame retardant material.

[0087] 4. Compression performance test

[0088] According to GB / T 1041-92 standard, aerogel samples were tested for compression performance using a universal strength tester. During the test, the compression rate was 10 mm min. -1 The strains of the aerogel samples were 10%, 20%, 30%, 50% and 70% respectively. The Young's modulus of the aerogel was calculated based on the slope of the linear interval of the curve. When the strain was 30%, the aerogel was subjected to repeated compression resilience tests for 100 cycles.

[0089] The test results are as follows:

[0090] 1. Preparation and morphology of UiO-66-NH2@ANF aerogel

[0091] The present invention limits the ligand to ATA and synthesizes UiO-66-NH2. The presence of amino groups is expected to improve its degradation performance. However, due to the inert surface of ANF, direct solvent thermal growth still results in poor MOF loading along the fiber. Therefore, the present invention pre-treats ANF with ATA. It is found that after treatment with ATA, the color of the ANF dispersion changes significantly, such as Figure 1 As shown ( Figure 1 (a) is ANF / DMF dispersion, (b) is ATA@ANF / DMF dispersion), the color changes from the original light yellow to light pink, indicating the attachment of ATA on the fiber surface.

[0092] In order to verify the promoting effect of ATA on the growth of UiO-66-NH2, the aerogel treated with ATA was characterized by infrared and XPS. Figure 2 Compared with ANF, ATA@ANF has a -1 , 1160cm -1 , 990cm-1 There is a significant change at 1700cm -1 The stretching vibration of C=O bond is 1160cm -1 and 990cm -1 It is caused by NH bonds. This shows that ATA is well attached to the surface of aramid nanofibers, providing nucleation sites for the subsequent growth of MOF.

[0093] In order to further prove the role of ATA, the present invention uses XPS to roughly compare the element contents in ANF and ATA@ANF. As shown in Table 1, the oxygen content in ATA@ANF is significantly higher than that in ANF, which also indirectly proves the attachment of carboxyl groups.

[0094] Table 1 XPS element contents of ANF and ATA@ANF aerogels

[0095]

[0096] A large amount of uniform UiO-66-NH2 was loaded on the ANF pretreated by ATA, and its morphology was observed by SEM. Figure 3 As shown in (a), it can be found that UiO-66-NH2 grows uniformly along the fiber without obvious agglomeration; TEM and mapping results ( Figure 3 (b) also further confirmed the uniformity of UiO-66-NH2 loading.

[0097] After loading UiO-66-NH2, ANF aerogel still maintains its lightweight characteristics, such as Figure 4 As shown. Calculation shows that the original aerogel density without UiO-66-NH2 is only 2.7 mg / cm 3 (where the ANF content is 0.25wt%), and the density of UiO-66-NH2@ANF aerogel loaded with UiO-66-NH2 is 4.7mg / cm 3 (wherein the ANF content is 0.25wt% and the UiO-66-NH2 loading is 106%).

[0098] 2. UiO-66-NH2 loading control

[0099] When regulating the loading amount of UiO-66-NH2 on ANF, the present invention firstly explored the effect of ATA pretreatment time on the loading of UiO-66-NH2. After calculation, after 0h, 0.5h and 4h treatment, the loading amount of UiO-66-NH2 on ANF was 43%, 65% and 106% respectively. It can be seen that the loading amount obtained by solvent thermal growth after 4h pretreatment was the largest. Then the present invention again regulated the effect of the addition amount of MOF precursor. The results are as follows Figure 5As shown in FIG. 1 , as the amount of MOF precursor added gradually increases, the amount of MOF growing along the fiber also increases. In addition, the present invention also calculates the loading amount of UiO-66-NH2 in detail and plots it into a curve as shown in FIG. Figure 6 As shown in the figure, the loading amounts of UiO-66-NH2@ANF-0h aerogel, UiO-66-NH2@ANF-0.5h aerogel and UiO-66-NH2@ANF-4h aerogel are 43%, 65% and 106%, respectively; the loading amounts of UiO-66-NH2@ANF-0.3 aerogel, UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel are 55%, 64%, 125% and 261%, respectively, and the variation pattern is consistent with the results observed by SEM.

[0100] The present invention selected three aerogels, UiO-66-NH2@ANF-2, UiO-66-NH2@ANF-1 and UiO-66-NH2@ANF-0.5, from the above samples and conducted a series of tests. In the following figure, the three aerogels are recorded as UiO-66-NH2@ANFA-X (where A refers to aerogel; X is the amount of MOF precursor added, X=2, 1, 0.5).

[0101] Figure 7 The Fourier transform infrared peak change diagram of UiO-66-NH2, UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel, UiO-66-NH2@ANF-2 aerogel and ANF aerogel. Figure 1 On the one hand, it proves the loading of UiO-66-NH2. On the other hand, the peak changes caused by different loading amounts are also different. -1 、1560cm -1 、1200cm -1 、764cm -1 There are obvious changes in the 3330cm -1 、1560cm -1 、1200cm -1 All of them are peak changes caused by carboxyl groups, 764cm -1 The peak vibration is caused by the Zr-O bond. In terms of peak intensity, compared with UiO-66-NH2@ANFA-0.5 and UiO-66-NH2@ANFA-1, the peak intensity of UiO-66-NH2@ANFA-2 is the most obvious, which corresponds to the fact that it has the most UiO-66-NH2.

[0102] Figure 8(a) is the thermogravimetric change diagram of UiO-66-NH2, UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel. The four samples showed roughly the same trend, with three obvious weight loss stages. The first weight loss occurred at around 100°C, where water and solvent were removed; the second weight loss occurred at around 300°C, due to the decomposition of unreacted 2-aminoterephthalic acid; the third weight loss was caused by structural collapse, with skeleton collapse beginning at 500°C and complete decomposition after 600°C. At 1000°C, the residual amounts of UiO-66-NH2, UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel were 43.16%, 53.85%, 50.54% and 46.14%, respectively. The more the loading amount, the less the final residual amount.

[0103] Figure 8 (b) is the X-ray diffraction pattern of UiO-66-NH2, UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel, UiO-66-NH2@ANF-2 aerogel and ANF aerogel. It can be observed that UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel have almost the same peak shape, and all have typical diffraction peaks at 7.27° and 8.4°, which are consistent with the diffraction peaks of conventionally synthesized UiO-66-NH2 powder.

[0104] In order to prove the catalytic activity of UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel, the present invention also carried out automatic specific surface area and porosity tests on them, such as Fig. 9 shown. Fig. 9 (a) shows the adsorption-desorption curves of the three samples. In the low pressure range, i.e., P / P0 < 0.1, a typical type I isotherm is presented, which is caused by the rich microporous structure brought by the loading of UiO-66-NH2; in the high pressure range, i.e., P / P0 > 0.9, a typical H4 type hysteresis loop is presented, which is attributed to the mesoporous structure of ANF. The rich microporous structures of UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel, and UiO-66-NH2@ANF-2 aerogel are Fig. 9This is also shown in (b). In addition, the present invention found that the microporous structures of UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel are significantly more than that of UiO-66-NH2@ANF-0.5 aerogel, which is also caused by the difference in the loading amount of UiO-66-NH2.

[0105] The present invention also counted the BET and average pore size of the three samples. As shown in Table 2, the BET of UiO-66-NH2@ANF-2 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-0.5 aerogel were 589.349 m 2 / g, 545.965m 2 / g, 381.319m 2 / g, and the average pore sizes are 1.503nm, 1.453nm, and 1.403nm respectively.

[0106] Table 2 BET and pore size analysis of UiO-66-NH2@ANF aerogel

[0107]

[0108] 3. Catalytic degradation performance

[0109] The reaction progress of UiO-66-NH2@ANF aerogel to CEES was monitored by gas chromatography (GC). Fig.10 The monitoring of gas chromatography at different reaction times was recorded in detail. The three aerogels all recorded the reaction conditions at 10min, 20min, 30min, 1h, 3h, 6h, 10h, 15h, 24h, 48h and 72h. It can be found that with the extension of time, the three aerogels showed the same change pattern, that is, the peak at 5.18 gradually increased, and the peak at 5.21 gradually weakened to almost nothing. Compared with pure CEES, it was found that the peak at 5.21 gradually disappeared was the CEES peak, which proved the removal of CEES by aerogel and the generation of new substances after the reaction. The CEES peak almost disappeared after 72 hours.

[0110] By fitting the peak area in the gas chromatography, the removal rate of CEES by UiO-66-NH2@ANF aerogel can be calculated. Unlike UiO-66@ANF aerogel, UiO-66-NH2@ANF aerogel shows a surprising effect in the degradation of mustard gas simulant CEES. According to the calculation results, the degradation rates of the three aerogels within 10 hours all reached more than 90%, which is much higher than that of UiO-66@ANF aerogel. The present invention further extended the time and found that after 72 hours, the degradation rates of CEES by the three aerogels, namely UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel, were 97%, 98.7% and 98.9%, respectively. Fig.11 As shown in (a). The degradation rate of UiO-66-NH2@ANF-2 aerogel is the highest, which corresponds to the previous BET result. In addition, compared with the protective materials reported in other literature, the degradation rate of UiO-66-NH2@ANF aerogel is much higher than that of these metal oxides and polyoxometalates, as shown in Table 3. The present invention also found that when these materials are used to degrade HD or CEES, the dosage is mostly around 100 mg or more, but the degradation rate is basically below 90%.

[0111] In addition to the higher degradation rate, the half-life of UiO-66-NH2@ANF aerogel is also much lower than that of UiO-66@ANF aerogel. Fig.11 (b) shows the half-life of UiO-66-NH2@ANFA-X (X = 0.5, 1, 2), which are 21.65 minutes, 10.5 minutes, and 8.15 minutes, respectively. Compared with other protective materials, UiO-66-NH2@ANF aerogel also has a greater advantage in half-life, as shown in Table 3.

[0112] Table 3 Degradation performance comparison table

[0113]

[0114] The degradation products were further detected by gas chromatography-mass spectrometry (GC-MS), such as Fig.12 As shown in (a), a total of three substances were detected: 2-chloroethyl ethyl sulfide (CEES), 2-hydroxyethyl sulfide (HEES) and 1,2-bis(ethylthio)ethane (BETE). Because the degradation rate did not reach 100%, trace amounts of CEES could still be detected. The causes of the formation of the other two products are shown in (b) and (c) in 12. The cause of the formation of HEES is shown in Fig.12 (b); The generation of BETE is because the highly active surface of UiO-66-NH2@ANF aerogel produces free radicals, which leads to the breakage of CC or CS bonds, thus forming BETE, such as Fig.12 Therefore, it can be determined that CEES reduces the toxicity of CWAs mainly through hydrolysis and fragment reassembly.

[0115] In practical applications, the protective material is not only required to have efficient and rapid degradation performance, but also to have a certain stability. Therefore, the present invention tests the reusability of UiO-66-NH2@ANF-1 aerogel. Fig.13 The present invention found that after being reused three times, the UiO-66-NH2@ANF-1 aerogel still retained a degradation rate of more than 94%. In order to further prove that the UiO-66-NH2@ANF-1 aerogel still has the original structure and performance after repeated use, the present invention conducted infrared and XRD tests on the samples after three repetitions, as shown in FIG. Fig.13 In (b-c), the morphology of UiO-66-NH2@ANF-1 aerogel after the third use was observed by SEM, such as Fig.13 Middle (d). Fig.13 The infrared spectrum of (b) shows that the UiO-66-NH2@ANF-1 aerogel after three times of CEES degradation is basically similar to the UiO-66-NH2@ANF-1 aerogel before degradation, except for the peaks at 1040-1290 cm -1 There are slight differences in the range, which are caused by decomposition products or residual CEES. Fig.13 The XRD in (c) shows that the degraded UiO-66-NH2@ANF-1 aerogel has the same peak shape as the undegraded UiO-66-NH2@ANF-1 aerogel, but the peak is slightly shifted to the left due to the influence of decomposition products and residual CEES. Fig.13 The SEM image in (d) also clearly shows that the morphology of the MOF crystal has not changed, indicating that its structure is stable, confirming its structural stability.

[0116] 4. Analysis of thermal insulation and flame retardant properties

[0117] In order to explore the flame retardant effect of UiO-66-NH2@ANF aerogel, the limiting oxygen index of UiO-66-NH2@ANF-0.5 aerogel and UiO-66-NH2@ANF-1 aerogel were tested respectively. The results showed that the limiting oxygen index of UiO-66-NH2@ANF-0.5 aerogel was 30, and the limiting oxygen index of UiO-66-NH2@ANF-1 aerogel was 32. It can be seen that the loading of UiO-66-NH2 is beneficial to the flame retardancy of aramid nanofiber aerogel.

[0118] In order to further explore the thermal insulation performance of UiO-66-NH2@ANF aerogel, the present invention prepared three UiO-66-NH2@ANF aerogels with different ANF concentrations, namely 0.25wt%, 0.20wt%, and 0.15wt%, and the height was controlled at 15mm. Fig.14 (a). The present invention firstly uses an infrared thermal imager to evaluate it, and places three concentrations of aerogels on a heating table at 200°C in the order of 0.25wt%, 0.20wt%, and 0.15wt% from left to right, and leaves them for 30 minutes. Fig.14 (b) shows the average temperature of the upper surface of the sample at 0min and 30min. It can be found that the temperature difference of the three samples did not change much within 30min. The upper surface temperatures of the four samples of 0.30wt%, 0.25wt%, 0.20wt%, and 0.15wt% were 91.3℃, 82.4℃, and 70.6℃ at 0min, and 97.4℃, 92.5℃, and 81.2℃ at 30min, respectively, with a temperature difference of 6.1℃, 10.1℃, and 10.6℃. Both the average temperature of the upper surface of the sample at 0min and at 30min showed a phenomenon of gradually increasing with the increase of sample concentration, and the maximum temperature difference of the three samples did not exceed 11℃, indicating that the sample temperature was relatively stable. Fig.14 The temperature change curve in (c) also intuitively shows this law. The surface temperature of the sample increases with concentration. This is because within a certain range, as the aerogel concentration, that is, the density, increases, the heat transfer inside the aerogel is mainly contact conduction, which makes its thermal insulation effect worse.

[0119] In order to further verify this result, the present invention also tested the thermal conductivity of the three concentrations of aerogels, such as Fig.14 As shown in (d), it is worth noting that the thermal conductivity of the three concentration samples is kept below 30mW / mK, which meets the requirements of thermal insulation materials. The thermal conductivity of UiO-66-NH2@ANF aerogels with concentrations of 0.15wt%, 0.20wt%, and 0.25wt% are 25.66mW / mK, 26.95mW / mK, and 28.14mW / mK, respectively, which is consistent with the above observations and records using the infrared thermal imager.

[0120] 5. Compression performance analysis

[0121] In order to study the structural stability of UiO-66-NH2@ANF-1 aerogel, the present invention conducted a compression performance test on it, such as Fig.15 As shown in the figure, the UiO-66-NH2@ANF-1 aerogel prepared in the present invention has excellent mechanical properties and can withstand considerable compression without causing structural collapse, which is very different from the fragile nature of typical porous cross-linked materials. Fig.15 As shown in (a), the UiO-66-NH2@ANF-1 aerogel was subjected to compression tests at strains of 10%, 20%, 30%, 50% and 70%, respectively. It can be seen from the figure that the compression process can be divided into three characteristic deformation stages. When the strain ε is less than 10%, it is called the linear or Hooke elastic zone. The stress σ in this stage remains basically unchanged. The deformation in this stage is mainly caused by the flexibility of the fiber. When 10% < ε < 60%, the stress increases linearly with the increase of strain, indicating that the internal structure of the aerogel is well maintained. When ε is greater than 60%, the gaps between the fibers inside the aerogel are highly compressed and become dense, resulting in a sharp increase in stress. However, the aerogel at this time can still maintain structural integrity, indicating that the bonding between the fibers through physical / chemical interactions is very strong. This phenomenon is consistent with the stress-strain curve of a typical elastic aerogel.

[0122] In order to further evaluate the compression resistance of UiO-66-NH2@ANF-1 aerogel, the present invention also studies its cyclic compression performance under 30% strain. The stress-strain curve of UiO-66-NH2@ANF-1 aerogel compressed 100 times is shown in Figure 2. Fig.15 As shown in (b), it can be seen that after 100 cycles, the compression curve is still a closed hysteresis loop, indicating that its structure is good. Moreover, after the stress is eliminated, the obtained aerogel can basically return to its initial position, with only slight irreversible deformation, and the height changes from the original 30mm to 28mm. Fig.15 The size retention rate in (c) is 93.3%, indicating that UiO-66-NH2@ANF aerogel has excellent structural stability and durability.

[0123] 6. Analysis of air permeability and moisture permeability

[0124] It is very necessary to study the air permeability and moisture permeability of UiO-66-NH2@ANF-1 aerogel, which will not only affect the comfort of the wearer, but also have a great impact on the degradation ability of chemical warfare agents. Generally speaking, the worse the air permeability, the worse the corresponding chemical warfare agent permeability, which can ensure that it is fully in contact with the active molecules, thereby improving its degradation. The air permeability of UiO-66-NH2@ANF-1 aerogel was tested to be 9.379mL·cm -2 ·s -1 , and ZORFLEX activated carbon cloth product HF70K up to 109mL·cm -2 ·s -1 Compared with the air permeability of ANF-1, the air permeability of UiO-66-NH2@ANF-1 aerogel is very poor, but it is helpful for the degradation of chemical warfare agents. At the same time, it can also reduce the penetration of chemical warfare agents and prevent pollution to the human body.

[0125] In addition to air permeability, the present invention also evaluates the moisture management ability of UiO-66-NH2@ANF-1 aerogel. Fig.16 As shown in Table 4, the blue part represents the salt water wetted area, and the dark part represents the area not wetted by salt water. The upper and lower surfaces of the aerogel show the same wetting pattern, indicating that it has good water permeability. At the same time, the salt water has poor diffusion on the aerogel. As shown in Table 4, the water expansion rates on the upper and lower surfaces of the aerogel are 0.4645 and 0.4141 mm s, respectively. -1 , and the diffusion radius is only 5 mm. To some extent, the damage range to the UiO-66-NH2@ANF-1 aerogel structure is minimal.

[0126] Table 4 Moisture management capability of UiO-66-NH2@ANF-1 aerogel

[0127]

[0128] The present invention discusses the preparation of UiO-66-NH2@ANF aerogel and its catalytic degradation of CEES and thermal insulation, compression and other properties. The present invention first discusses the in-situ growth of UiO-66-NH2 on ANF under different conditions, including solvent thermal growth after ATA pretreatment for different times and solvent thermal growth after adding different amounts of MOF precursors after the same pretreatment time. After determining the treatment conditions, the catalytic degradation performance of UiO-66-NH2@ANF aerogel on mustard gas simulant CEES was systematically studied, and then the flame retardant and thermal insulation properties of UiO-66-NH2@ANF aerogel were studied. Finally, the compression performance of UiO-66-NH2@ANF aerogel was explored. The following conclusions are obtained:

[0129] (1) The loading of UiO-66-NH2 on ANF was different when ATA was used to treat ANF for different time periods. The results showed that the loading of UiO-66-NH2 on the aerogel was optimal after ATA treatment for 12 hours.

[0130] (2) Under the premise of ATA pretreatment of ANF for 12 hours, the amount of MOF precursor added was adjusted. The results showed that when the amount of MOF precursor added was twice that of ANF, there was still no obvious agglomeration phenomenon, and UiO-66-NH2 grew very uniformly along the fiber, with a loading capacity of up to 261%.

[0131] (3) The degradation experiment of CEES on UiO-66-NH2@ANF aerogel showed that the degradation ability of UiO-66-NH2@ANF aerogel on CEES was much higher than that of UiO-66@ANF aerogel. The degradation rates of CEES of three ANF aerogels with different loadings, namely UiO-66-NH2@ANF-0.5 aerogel, UiO-66-NH2@ANF-1 aerogel and UiO-66-NH2@ANF-2 aerogel, were 97%, 98.7% and 98.9%, respectively, and the half-lives were 21.65 minutes, 10.5 minutes and 8.15 minutes, respectively. Compared with some other typical materials, UiO-66-NH2@ANF aerogel has great advantages in both degradation rate and half-life. GC-MS verification showed that the products of CEES degradation by UiO-66-NH2@ANF aerogel included 2-hydroxyethyl ethyl sulfide (HEES) and 1,2-bis(ethylthio)ethane (BETE).

[0132] (4) UiO-66-NH2@ANF aerogel has a certain structural stability. After repeated degradation of CEES, the structure of UiO-66-NH2@ANF aerogel remains stable, and the degradation rate remains above 94% after three degradations.

[0133] (5) UiO-66-NH2@ANF aerogel has excellent flame retardancy, and the more UiO-66-NH2 is loaded, the better the flame retardant effect is; the highest limiting oxygen index is greater than 30, which is a flame-retardant material.

[0134] (6) UiO-66-NH2@ANF aerogel has excellent thermal insulation properties and a thermal conductivity as low as 25.66 mW / mK.

[0135] (7) UiO-66-NH2@ANF aerogel has good compression performance and does not collapse even under very high strain conditions. After 100 cycles of compression at 30% strain, the stress-strain curve is still a closed hysteresis loop with a recovery rate of 93.3%, indicating that its structure is good.

[0136] (8) The air permeability test of UiO-66-NH2@ANF aerogel showed that the air permeability was 9.37 cm -3 cm -2 ·s -1 , the air permeability is poor, indicating that CEES can stay in the aerogel for a long time during the permeation process, ensuring contact with UiO-66-NH2 molecules, which is conducive to the degradation of CEES. In addition, the MMT test of UiO-66-NH2@ANF aerogel shows that the water permeability is very good and will not diffuse, with a diffusion radius of only 5mm.

[0137] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A MOF-containing aramid aerogel, characterized in that: The MOF-loaded aramid nanofiber aerogel comprises MOF and aramid nanofibers; the loading amount of the MOF is 60-270%; the MOF is UiO-66-NH2; the MOF-loaded aramid nanofiber aerogel has a thermal conductivity of less than 30 mW / mk and a specific surface area of ​​280-590 m 2 / g, pore volume is 0.25-0.35cm 3 / g, and the average pore size is 1.4-1.6nm.

2. A method for preparing the MOF-containing aramid aerogel according to claim 1, characterized in that: The following steps are involved: Step 1, placing aramid nanofibers in N,N-dimethylformamide to prepare an ANF / DMF dispersion, then adding 2-aminoterephthalic acid and stirring to obtain a pre-reaction solution; Step 2, adding MOF precursor and glacial acetic acid to the pre-reaction solution and mixing them evenly to obtain a reaction solution; Step 3, subjecting the reaction solution to a solvothermal reaction, followed by washing and replacing the solvent to obtain an aramid nanofiber solution loaded with MOF; Step 4, adding tert-butyl alcohol, water and blocked isocyanate to the MOF-loaded aramid nanofiber solution to prepare a dispersion, followed by freeze-drying and activation to obtain the MOF-loaded aramid nanofiber aerogel.

3. The preparation method according to claim 2, characterized in that: In step 1, the concentration of the ANF / DMF dispersion is 0.4wt%; the mass ratio of the aramid nanofiber to the 2-aminoterephthalic acid is 1:

1.

4. The preparation method according to claim 2, characterized in that: In step 2, the MOF precursor is a mixture of zirconium salt and 2-aminoterephthalic acid in a molar ratio of 1:1; the mass ratio of the MOF precursor to the aramid nanofiber is 0.3-2:1; the molar ratio of the glacial acetic acid to the zirconium salt is 200:1; the stirring is specifically: stirring at room temperature for 0.5-4h; the zirconium salt is zirconium chloride.

5. The preparation method according to claim 2, characterized in that: In step 3, the solvent thermal reaction is specifically: reacting at 120° C. for 12 hours; washing with DMF and methanol; and replacing the solvent with water.

6. The preparation method according to claim 2, characterized in that: In step 4, the volume ratio of tert-butyl alcohol to water is 1:10; the amount of blocked isocyanate added is 0.1% of the content of aramid nanofibers; and the concentration of MOF-loaded aramid nanofibers in the dispersion is 0.15-0.25wt%.

7. The preparation method according to claim 2, characterized in that: In step 4, the freeze-drying step also includes a freeze-molding step.

8. The preparation method according to claim 2, characterized in that: In step 4, the activation is specifically performed under vacuum conditions at 80° C. for 12 hours.

9. Use of the MOF-containing aramid aerogel as claimed in claim 1 in carbon dioxide adsorption.

Citation Information

Cited By

  • UiO-67-SO2-coated ANF fiber aerogel as well as preparation method and application thereof

    CN119327430A

  • UiO-67-so2@anf fiber aerogel and preparation method and application thereof

    CN119327430B

  • UiO-66-NH2-F4-coated ANF fiber aerogel as well as preparation method and application thereof

    CN119327431A

  • UiO-66-nh2-f4@anf fiber aerogel, and preparation method and application thereof

    CN119327431B