Method for producing walling material by using papermaking white mud
A technology for paper-making lime mud and wall materials, which is applied in solid waste management, sustainable waste treatment, climate sustainability, etc., can solve the problems of clogging equipment, high production costs, threatening food production, etc., and reduce production energy consumption. and cost, low cost of industrialized operation, and the effect of promoting sustainable development
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2013-09-04
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 1 
Figure 2 
Figure 3
Abstract
Description
technical field
[0001] The invention belongs to a method for preparing block-like or other-shaped building components in building components, and relates to a method for mainly using waste to prepare building wall materials—blocks, and in particular to a method for producing wall materials using papermaking white mud method. It is suitable for mainly using waste papermaking white mud, lithium slag, etc. to produce building wall materials - blocks. Background technique
[0002] Papermaking white mud (hereinafter referred to as white mud) comes from the white mud recovery stage of the alkali recovery workshop in the papermaking process; in the papermaking process, the pulping black liquor is extracted, evaporated and concentrated, and roasted in the alkali recovery furnace to obtain the melt. Dissolve in water to form a green liquid, then add lime to the green liquid for causticization reaction to obtain a white precipitate, which is white mud.
[0003] In papermaking lime m...
Examples
Embodiment 1
[0036] A method for producing wall materials using papermaking white mud, comprising the following steps:
[0037] 1) By weight percentage, take 43.5% of white mud, 45% of lithium slag, 10% of PO42.5 cement, and 1.5% of active stimulating agent (RDDM). Add to the mixer and mix for 3 minutes, then pour into the mold, and vibrate 120 times on the vibrating table to form;
[0038] 2) Put the mold in a curing box with a temperature of 20±1°C and a humidity of 91% for 20 hours, then remove the mold, and then put it in a curing box with a temperature of 65°C for 20 hours to obtain the wall material.
Embodiment 2
[0040] A method for producing wall materials using papermaking white mud, comprising the following steps:
[0041] 1) In terms of percentage by weight, take 48.9% of white mud, 30% of lithium slag, 20% of PO42.5 cement, and 1.1% of active activator (RDDM), mix it in a mixer for 5 minutes, then pour it into the mold, and 80 vibrations on the vibrating table for forming;
[0042] 2) Put the mold in a curing box with a temperature of 20±1°C and a humidity of 92% for 24 hours, then remove the mold, and then put it in a curing box with a temperature of 65°C for 30 hours to obtain the wall material.
Embodiment 3
[0044] A kind of method utilizing white mud to produce wall body material is characterized in that: it comprises:
[0045] 1) By weight percentage, take 58.2% of white mud, 20% of lithium slag, 20% of PO42.5 cement, 1.8% of active stimulating agent (RDDM), mix in a mixer for 10 minutes, then pour into the mold, and 60 vibrations on the vibrating table for forming;
[0046] 2) Put the mold in a curing box with a temperature of 20±1°C and a humidity of 95% for 30 hours, then remove the mold, and then put it in a curing box with a temperature of 65°C for 24 hours to obtain the wall material.
[0047] The wall body brick that the wall body material that this example is made is made by autoclave method, through measuring, the mechanical property of excellent product is as follows:
[0048]