Sludge powder nano soft soil modifier and preparation method thereof
A modifier and nanotechnology, applied in the field of silt powder nanosoft soil modifier and its preparation, can solve the problems of low tensile strength, slow strength growth, poor toughness, etc.
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2017-11-07
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 1
Abstract
Description
technical field
[0001] The invention belongs to the field of sludge treatment, and in particular relates to a sludge powder nanometer soft soil modifier and a preparation method thereof. Background technique
[0002] With the rapid increase of urban population and the rapid development of society and economy, a large amount of untreated production wastewater and domestic sewage are discharged into the inner lake. Over the years, a thick layer of sediment is deposited on the riverbed and the bottom of the lake. This has led to serious pollution from both inside and outside the city, increasing eutrophication of water bodies, and declining water quality, which has greatly affected the ecological environment of the city and the living environment of residents. Contradictions such as river siltation and environmental problems have become increasingly prominent. How to dispose of river silt, find the most feasible and effective solution, realize the comprehensive utilization o...
Examples
Embodiment 1
[0023] A silt powder nano-soft soil modifier, made of the following raw materials in parts by weight: 1.8 parts of P.O 42.5R ordinary Portland cement, 2.3 parts of S95 granulated blast furnace slag, 1.8 parts of CL90 quicklime, F.II grade powder 0.6 parts of coal ash, 0.5 parts of nano-scale silica powder, 0.6 parts of composite activator, 0.4 parts of sepiolite fiber, 0.8 part of alkali-resistant glass fiber, 0.8 part of wollastonite fiber, and 1.2 parts of papermaking white mud.
[0024] The composite activator is made by mixing polyacrylic acid, polycarboxylate water reducer, aluminum potassium sulfate, calcium sulfate, sodium sulfate and magnesium sulfate in a weight ratio of 100:15:13:5:4:1.
[0025] The preparation method of the composite activator is as follows: heat polyacrylic acid to 70°C, add polycarboxylate water reducer, stir for 13 minutes, then add aluminum potassium sulfate, calcium sulfate, sodium sulfate and magnesium sulfate, and stir for 5 minutes, That is,...
Embodiment 2
[0030] A silt powder nano-soft soil modifier, made of the following raw materials in parts by weight: 1.9 parts of P.O 42.5R ordinary Portland cement, 2.2 parts of S95 granulated blast furnace slag, 1.9 parts of CL90 quicklime, F.II grade powder 0.5 parts of coal ash, 0.6 parts of nano-scale silica powder, 0.6 parts of composite activator, 0.4 parts of sepiolite fiber, 0.7 part of alkali-resistant glass fiber, 0.9 part of wollastonite fiber, and 1.0 part of papermaking white mud.
[0031] The composite activator is made by mixing polyacrylic acid, polycarboxylate water reducer, aluminum potassium sulfate, calcium sulfate, sodium sulfate and magnesium sulfate in a weight ratio of 100:17:10:6:3:2.
[0032] The preparation method of the composite activator is as follows: heat polyacrylic acid to 72°C, add polycarboxylate water reducer, stir for 11 minutes, then add aluminum potassium sulfate, calcium sulfate, sodium sulfate and magnesium sulfate, and stir for 7 minutes, That is, ...
Embodiment 3
[0037] A silt powder nano-soft soil modifier, made of the following raw materials in parts by weight: 2.0 parts of P.O 42.5R ordinary Portland cement, 2.1 parts of S95 granulated blast furnace slag, 2.0 parts of CL90 quicklime, F.II grade powder 0.5 parts of coal ash, 0.6 parts of nano-scale silica powder, 0.5 parts of composite activator, 0.5 parts of sepiolite fiber, 0.6 part of alkali-resistant glass fiber, 1.0 part of wollastonite fiber, and 0.8 part of papermaking white mud.
[0038] The composite activator is made by mixing polyacrylic acid, polycarboxylate water reducer, aluminum potassium sulfate, calcium sulfate, sodium sulfate and magnesium sulfate in a weight ratio of 100:20:7:7:3:3.
[0039] The preparation method of the composite activator is: heating polyacrylic acid to 75°C, adding polycarboxylate water reducer, stirring for 10 minutes, then adding aluminum potassium sulfate, calcium sulfate, sodium sulfate and magnesium sulfate, and stirring for 10 minutes, Tha...