Dyeing method for acrylic top
A dyeing method and technology for wool tops, which are applied in dyeing methods, textiles and papermaking, etc., can solve problems such as easy to produce color flowers, poor dyeing uniformity, and low color fastness of dyed wool tops, and achieve excellent light color fastness, Optimal dyeing effect and good dyeing uniformity
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2017-01-11
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to a method for dyeing acrylic wool tops. Background technique
[0002] In the existing method for dyeing acrylic wool tops, the color fastness of the dyed wool tops is not high, the dyeing uniformity is not good, and colored flowers are easy to occur. Contents of the invention
[0003] The purpose of the present invention is to provide a method for dyeing acrylic wool tops, the dyed wool tops have excellent light fastness, washing color fastness, dry cleaning color fastness, rubbing color fastness, perspiration color fastness, water stain Color fastness, color fastness to chlorine bleaching, color fastness to non-chlorine bleaching, and good dyeing uniformity, colorless flowers.
[0004] In order to achieve the above object, the technical solution of the present invention is to design a kind of dyeing method of acrylic wool top, comprising the steps:
[0005] 1) Add 1 to 2 parts by weight of secondary alcohol polyoxyethylene ...
Examples
Embodiment 1
[0039] The dyeing method of acrylic wool top, comprises the steps:
[0040] 1) Add 1 to 2 parts by weight of secondary alcohol polyoxyethylene ether, 0.7 parts by weight of triallylamine, 1.9 parts by weight of natron, 1.8 parts by weight of diethylaminoethyl methacrylate, 30 parts by weight 100 parts by weight of vegetable dyes are dropped into 100 parts by weight of deionized water, stirred evenly, and heated to 45°C;
[0041] 2) Add 2.9 parts by weight of polyaspartic acid, 0.7 parts by weight of sodium dodecylsulfonate, 0.4 parts by weight of zinc stearate, and 2.6 parts by weight of α-alanine in turn, and continue to stir until fully mixed. and heated to 60°C;
[0042] 3) Soak the top in the dye vat for 50 minutes;
[0043] 4) drying the soaked tops at 85°C;
[0044] 5) immerse the dried top in clear water and rinse for 50 minutes;
[0045] 6) Take out the wool top after rinsing and let it dry naturally.
Embodiment 2
[0047] The dyeing method of acrylic wool top, comprises the steps:
[0048] 1) Add 1 part by weight of secondary alcohol polyoxyethylene ether, 0.7 part by weight of triallylamine, 1.9 parts by weight of natron, 1.8 parts by weight of diethylaminoethyl methacrylate, 30 parts by weight of plant Add 100 parts by weight of deionized water to the dye in turn, stir evenly, and heat to 45°C;
[0049] 2) Add 2.9 parts by weight of polyaspartic acid, 0.7 parts by weight of sodium dodecylsulfonate, 0.4 parts by weight of zinc stearate, and 2.6 parts by weight of α-alanine in turn, and continue to stir until fully mixed. and heated to 60°C;
[0050] 3) Soak the top in the dye vat for 50 minutes;
[0051] 4) drying the soaked tops at 85°C;
[0052] 5) immerse the dried top in clear water and rinse for 50 minutes;
[0053] 6) Take out the wool top after rinsing and let it dry naturally.
Embodiment 3
[0055] The dyeing method of acrylic wool top, comprises the steps:
[0056] 1) In the dye vat, add 2 parts by weight of secondary alcohol polyoxyethylene ether, 0.7 parts by weight of triallylamine, 1.9 parts by weight of natron, 1.8 parts by weight of diethylaminoethyl methacrylate, and 30 parts by weight of plant Add 100 parts by weight of deionized water to the dye in turn, stir evenly, and heat to 45°C;
[0057] 2) Add 2.9 parts by weight of polyaspartic acid, 0.7 parts by weight of sodium dodecylsulfonate, 0.4 parts by weight of zinc stearate, and 2.6 parts by weight of α-alanine in turn, and continue to stir until fully mixed. and heated to 60°C;
[0058] 3) Soak the top in the dye vat for 50 minutes;
[0059] 4) drying the soaked tops at 85°C;
[0060] 5) immerse the dried top in clear water and rinse for 50 minutes;
[0061] 6) Take out the wool top after rinsing and let it dry naturally.