Cover glass laminated structure

By using hardened layers of 2 to 10 μm thickness and other functional layers in the cover glass laminate structure, the problem of thinning of the decorative film layer in electronic products is solved, and the effect of low fracture, few bubbles and low wrinkles is achieved, satisfying the effect of Thin and lighten trends and improve user experience.

CN108000989BActive Publication Date: 2024-12-03ANHUI JINGZHUO OPTICAL DISPLAY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201610931674.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2016-10-31
Publication Date
2024-12-03
Estimated Expiration
2036-10-31

AI Technical Summary

Technical Problem

In electronic products with touch control functions, how to use a thinner decorative film layer to meet the needs of thinning and lightening while maintaining the physical properties of the film layer?

Method used

The cover glass laminated structure with a hardened layer thickness of 2 to 10 μm is adopted, combined with the UV texture layer, vapor deposition layer and ink layer, and the laminated structure of the bonding layer and the decorative layer can reduce the poor fit bubbles and wrinkles, and optimize the sticking of the glass substrate. Combination process.

Benefits of technology

It achieves the effect of low fracture, less bubbles and low wrinkles between the hardened layer and the glass substrate, thins the overall thickness, meets the thinning and lightening needs of electronic products, and improves user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108000989B_ABST
    Figure CN108000989B_ABST
Patent Text Reader

Abstract

The present invention relates to a cover glass laminate structure, comprising: a glass substrate, including an inner surface, and an outer surface spaced from the inner surface; an adhesive layer, adhered to the inner surface provided with the glass substrate; and a hardening layer, formed on a surface of the adhesive layer away from the glass substrate; wherein the thickness of the hardening layer is 2 to 10 μm; and the thickness of the adhesive layer is 5 to 100 μm. The present invention adopts a cover glass laminate structure without a PET substrate, wherein the thickness of the hardening layer is 2 to 10 μm, which can ensure fewer laminating bubbles and lower wrinkle defects. Furthermore, it is more preferred that the thickness of the hardening layer is greater than or equal to 2 μm and less than 5 μm, which can achieve the effect of lower fold defects, fewer laminating bubbles and lower wrinkle defects during the laminating process between the hardening layer and the glass substrate, thereby reducing the overall thickness of the cover glass laminate structure, thereby meeting the trend of thinning and lightening of electronic products with touch functions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of touch control technology, and in particular to a cover glass laminate structure applied to a touch control product. Background Art

[0002] At present, cover glass is widely used in electronic products with touch functions. Usually, multiple decorative film layers are set on the cover glass to make the cover glass meet specific appearance requirements. This traditional decorative film layer with PET substrate can be bonded to the surface of the cover glass through an adhesive layer.

[0003] In order to meet the demand for thinner and lighter electronic products with touch functions, thinner decorative film layers are used. How to use thinner decorative film layers without losing the physical properties of the decorative film layers is an urgent problem to be solved in this industry. Summary of the invention

[0004] Based on this, it is necessary to provide a cover glass laminate structure that can solve the above problems.

[0005] A cover glass laminate structure, comprising:

[0006] A glass substrate comprising an inner surface and an outer surface spaced apart from the inner surface;

[0007] An adhesive layer is attached to the inner surface of the glass substrate;

[0008] A hardening layer formed on a surface of the bonding layer away from the glass substrate;

[0009] Wherein, the thickness of the hardening layer is 2-10 μm; the thickness of the bonding layer is 5-100 μm.

[0010] In one embodiment, the thickness of the hardened layer is greater than or equal to 2 μm and less than 5 μm.

[0011] In one embodiment, the thickness of the adhesive layer is 5-20 μm.

[0012] In one of the embodiments, the cover glass laminate structure further includes a UV texture layer, a vapor deposition layer and an ink layer, and the hardened layer, UV texture layer, vapor deposition layer and ink layer are stacked in sequence.

[0013] In one embodiment, the UV texture layer can form brushed texture, CD texture or wavy texture.

[0014] In one embodiment, the cover glass laminate structure further includes a decorative layer, and the decorative layer is formed between the glass substrate and the bonding layer.

[0015] In one embodiment, the decoration layer is formed by silk screen printing.

[0016] In one embodiment, the decoration layer is a black ring, characters or icons.

[0017] In one embodiment, when the decoration layer is a black ring, the black ring is an annular structure with a circular through hole.

[0018] In one embodiment, the glass substrate has at least a partially curved surface.

[0019] The cover glass laminate structure provided by the present invention has at least the following advantages:

[0020] The present invention adopts a cover glass laminate structure without a PET substrate, and the cover glass laminate structure includes a hardened layer with a thickness of 2 to 10 μm, which can ensure fewer laminating bubbles and fewer wrinkles. Furthermore, it is more preferred that the thickness of the hardened layer is greater than or equal to 2 μm and less than 5 μm. This more preferred thickness can achieve the effects of lower folding defects, fewer laminating bubbles and lower wrinkles during the laminating process between the hardened layer and the glass substrate, thereby reducing the overall thickness of the cover glass laminate structure, thereby meeting the trend of thinning and lightening of electronic products with touch functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram of a cover glass stacking structure according to an embodiment of the present invention;

[0022] Figure 2 A schematic diagram of a cover glass stacking structure according to another embodiment of the present invention;

[0023] Figure 3 A schematic diagram of a glass substrate structure according to an embodiment of the present invention;

[0024] Figure 4 A schematic side view of a glass substrate according to an embodiment of the present invention;

[0025] Figure 5 This is a schematic diagram of a glass substrate structure according to another embodiment of the present invention;

[0026] Figure 6 This is a schematic diagram of a glass substrate structure according to another embodiment of the present invention;

[0027] Figure 7 This is a schematic diagram of a glass substrate structure according to another embodiment of the present invention;

[0028] Figure 8 for Figure 7 A schematic side view of the curved glass panel along the W direction is shown;

[0029] Fig. 9 for Figure 8 The schematic cross-sectional view of the curved glass panel along line AA is shown;

[0030] Fig.10 for Figure 7 The end view of the curved glass panel along the L direction is shown;

[0031] Fig.11 for Fig.10 A schematic cross-sectional view of the curved glass panel along line BB is shown. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0034] A cover glass laminate structure provided by the present invention can be used as a display surface shell of electronic products with touch function, and these electronic products include but are not limited to mobile phones, cameras, tablet computers, terminal displays, etc.

[0035] Figure 1 This is a schematic diagram of a cover glass stacking structure according to an embodiment of the present invention. Figure 1 The cover glass laminate structure includes a glass substrate 10 , an adhesive layer 40 and a hardening layer 50 .

[0036] The cover glass laminate structure further includes a UV texture layer 60 , a vapor deposition layer 70 and an ink layer 80 . The hardening layer 50 , the UV texture layer 60 , the vapor deposition layer 70 and the ink layer 80 are sequentially laminated.

[0037] The glass substrate 10 has an inner surface 101 and an outer surface 102 opposite to each other. Specifically in this embodiment, the glass substrate 10 is a flat glass. The glass substrate 10 can be in a rectangular, circular, square or other shape depending on the electronic product to which it is applied.

[0038] In this embodiment, the inner surface 101 of the glass substrate 10 is the surface facing the inside of the electronic product, and the outer surface 102 is the surface facing the user. In some embodiments, according to the requirements of anti-reflection, anti-fingerprint, etc. of the electronic product, a functional film layer such as an anti-reflection film and an anti-fingerprint film can be set on the outer surface 102 of the glass substrate 10. In addition, the glass substrate 10 can also be strengthened, and a hardened film layer can be set on any surface of the glass substrate 10.

[0039] The adhesive layer 40 is adhesive and very thin. Specifically in this embodiment, the adhesive layer 40 is an optically clear adhesive (OCA). The adhesive layer 40 is attached to the inner surface 101 of the glass substrate 10. Specifically in this embodiment, the thickness of the adhesive layer 40 is 5 to 100 μm. More preferably, the thickness of the adhesive layer 40 is 5 to 20 μm.

[0040] The hardening layer 50 is formed on a surface of the bonding layer 40 that is away from the glass substrate 10. As shown in Table 1, evaluation results of the hardening layer 50 of Examples 1 to 7 are given.

[0041] Table 1

[0042] Hardened layer thickness Poor fracture Poor fitting of bubbles and wrinkles Example 1 0.5μm 22.5% 0.2% Example 2 1μm 13.4% 0.4% Example 3 2μm 5.1% 0.7% Example 4 3μm 1.7% 1.1% Example 5 5μm 0.9% 1.6% Example 6 10μm 0.3% 5.3% Example 7 20μm 0.1% 20.8%

[0043] The degree of folding is proportional to the thickness of the hardened layer, that is, the thinner the hardened layer is, the more likely it is that folding will occur when the hardened layer is bonded to the glass substrate.

[0044] Poor lamination of bubbles and wrinkles is proportional to the thickness of the hardened layer, that is, the thicker the hardened layer, the easier it is for bubbles or wrinkles to appear when the hardened layer is laminated to the glass substrate.

[0045] As shown in Table 1, in Examples 1 and 2, the hardened layer is too thin, and the hardened layer is closely attached to the glass substrate, and bubbles or wrinkles are not easy to appear, but folds are easy to appear. Therefore, when the hardened layer thickness in Example 1 is 0.5 μm, the fold defect rate is as high as 22.5%, while the lamination bubble and wrinkle defect rate is as low as 0.2%; when the hardened layer thickness in Example 2 is 1 μm, the fold defect rate reaches 13.4%, while the lamination bubble and wrinkle defect rate is 0.4%.

[0046] As shown in Table 1, when comparing Examples 1 to 7, it is confirmed that the hardened layer thickness of 2 to 10 μm shown in Examples 3 to 6 is more preferred. This preferred thickness can ensure that the folding defect is within an allowable range, while also ensuring fewer bonding bubbles and lower wrinkle defects.

[0047] When comparing Examples 1 to 6, it is confirmed that the thickness of the hardened layer shown in Examples 3 to 5 is greater than or equal to 2 μm and less than 5 μm, which is more preferred. This more preferred thickness can achieve the effects of lower folding defects, fewer bonding bubbles and lower wrinkles during the bonding process of the hardened layer and the glass substrate, thereby thinning the overall thickness of the cover glass laminate structure, thereby meeting the trend of thinning and lightweight electronic products with touch functions.

[0048] The UV texture layer 60 is UV transferred onto the hardening layer 50. Specifically, when forming the UV texture layer 60, UV glue can be coated on the hardening layer 50, and then the UV glue can be embossed by a template to give the UV glue a specific pattern, such as setting a specific pattern such as a brushed pattern, a CD pattern or a wavy pattern on the UV glue layer, and then a mask is applied to cure and clean the uncured UV glue, so that the UV texture layer 60 formed on the hardening layer 50 can be obtained.

[0049] The vapor deposition layer 70 is disposed on the UV texture layer 60, and the vapor deposition layer 70 may be, for example, a film layer showing a metallic color. With the pattern of the UV texture layer 60 as a foil, an appearance with different patterns and colors can be observed on one side of the outer surface 102 of the glass substrate 10, showing a metallic texture, thereby significantly improving the display effect of characters or icons and enhancing the user experience.

[0050] After the UV texture layer 60 is further provided with the vapor deposition layer 70 and other structures, since the vapor deposition layer 70 is non-transparent and the UV texture layer 60 is transparent, the patterns presented by the UV texture layer 60 and the vapor deposition layer 70 can still be observed on the outer surface 102 of the glass substrate 10 .

[0051] The ink layer 80 is disposed on the evaporation layer 70. Both the ink layer 80 and the evaporation layer 70 are opaque, so when observing from the outer surface 102 toward the inner surface 101, the scene on the other side of the glass substrate 10 blocked by the ink layer 80 and the evaporation layer 70 cannot be seen.

[0052] The cover glass laminate structure also includes a decorative layer 30, which is formed between the glass substrate 10 and the bonding layer 40. Specifically, the decorative layer 30 is formed by silk screen printing. Specifically in this embodiment, the decorative layer 30 is a black ring, which is a ring structure with a circular through hole. The black ring is directly formed on the glass substrate, avoiding the visual impact caused by the camera alignment error. In this way, the process can be simplified to reduce the alignment error, effectively improve the yield of the product, and at the same time, the visual impact caused by the camera alignment error is avoided, thereby improving the user experience. It can be understood that in other embodiments, the decorative layer 30 can be a character or icon, which is directly formed on the glass substrate by silk screen printing. Compared with the direct exposure, development and silk screen printing method to obtain characters or icons, there will be defects such as tooth edge sawtooth. The method provided by the present invention can effectively reduce the defects caused by the direct exposure and development of the decorative layer such as characters or icons, thereby effectively improving the yield of the product.

[0053] Figure 2 This is a schematic diagram of a cover glass stacking structure according to another embodiment of the present invention. Figure 2 The cover glass laminate structure includes a glass substrate 20 , a bonding layer 40 and a hardening layer 50 .

[0054] The cover glass laminate structure further includes a UV texture layer 60 , a vapor deposition layer 70 and an ink layer 80 . The hardening layer 50 , the UV texture layer 60 , the vapor deposition layer 70 and the ink layer 80 are sequentially laminated.

[0055] See also Figure 3 The glass substrate 20 includes a plane portion 21 and a curved portion 22 extending from two opposite edges of the plane portion 21 and bending toward the same side surface of the plane portion 21. It can be understood that in other embodiments, all four edges of the glass substrate 20 can extend to form the curved portion 22, or only one edge of the glass substrate 20 can extend the curved portion 22.

[0056] Please also read Figure 4More specifically, the glass substrate 20 includes an inner surface 201, an outer surface 202 spaced apart from the inner surface 201, and a lateral surface 203 connecting the outer surface 202 and the inner surface 201. The inner surface 201 refers to a concave surface, and the outer surface 202 refers to a convex surface. Both the inner surface 201 and the outer surface 202 have a middle area and an edge area. In this embodiment, the plane portion 21 defines the middle area, and the curved surface portion 22 defines the edge area, that is, the plane portion 21 is located in the middle area, and the curved surface portion 22 is located in the edge area. In other embodiments, the edge area may also surround the middle area. For example, when the four edges of the glass substrate 20 are extended to form the curved surface portion 22, the middle area is surrounded by the edge area.

[0057] The inner surface 201 also includes a plane portion 211 and a curved portion 221 extending from two opposite edges of the plane portion 211 and bending toward one side. The two curved portions 221 are symmetrically arranged relative to the plane portion 211. The cross-section of the curved portion 221 is an arc. The radii of the two curved portions 221 may be equal or unequal. In the present embodiment, the radii of the two curved portions 221 are equal. The radii of the two curved portions 221 are 1 to 50 mm, preferably 5 to 50 mm, further preferably 5 to 20 mm, and more preferably 5 to 10 mm. The smaller the radius, the steeper the arc surface, and thus the formed glass substrate 20 has a stronger 3D stereoscopic effect in appearance.

[0058] The outer surface 202 also includes a plane portion 212 and a curved portion 222 extending from two opposite edges of the plane portion 212 and bent toward one side. Among them, the curved portion 222 of the outer surface 202 and the curved portion 221 of the inner surface 201 are bent toward the same side, that is, bent toward one side of the inner surface 201. The two curved portions 222 are symmetrically arranged relative to the plane portion 212. The cross-section of the curved portion 222 is an arc. The radii of the two curved portions 222 can be equal or unequal. In this embodiment, the radii of the two curved portions 222 are equal. The radii of the two curved portions 222 are 1 to 50 mm, preferably 5 to 50 mm, further preferably 5 to 20 mm, and more preferably 5 to 10 mm.

[0059] The plane portion 212 and the plane portion 211 correspond in position and have the same size, so when the outer surface 202 of the glass substrate 20 is placed on a horizontal plane, the orthographic projections of the plane portion 211 and the plane portion 212 on the horizontal plane completely overlap.

[0060] More specifically, the radii of the curved surface portion 222 and the curved surface portion 221 are also equal. In this embodiment, the distance between the inner surface 201 and the outer surface 202, that is, the thickness of the glass substrate 20 is 0.2 - 1.0 mm. The thickness of the glass substrate 20 is consistent everywhere, so that stress concentration can be better eliminated and the overall strength can be improved. Preferably, the thickness of the glass substrate 20 is 0.5 - 0.7 mm.

[0061] The included angle between the tangent line of the outermost edge point of the arc where the curved surface portion 222 is located and the plane portion 212 is defined as the C angle, and 0° < C < 90°, preferably 0° < C < 45°. The C angle between the curved surface portion 221 and the plane portion 211 can also have the same setting.

[0062] Furthermore, the distance between the outermost edge point of the arc where the curved surface portion 221 is located and the plane portion 212, that is, the height H of the glass substrate 20 is 0.5 - 5 mm.

[0063] In some embodiments, the orthographic projection of the glass substrate 20 on the horizontal plane is a rectangle, where the length of the rectangle is 50 - 500 mm and the width is 30 - 300 mm. The curved surface portions 221 and 222 are provided at the two edges where the length of the rectangle is located.

[0064] Figures 2 to 4 In the illustrated embodiment, the curved surface portion 22 extends out by bending from the opposite two sides of the plane portion 21 towards one side. In other embodiments, it can also extend out by bending from the four sides of the plane portion 21 towards one side to form an arc-shaped curved surface portion 22. The radii of the curved surface portions 22 extended from the opposite two sides can be equal or unequal. The radii of the curved surface portions 22 extended from the adjacent two sides can be equal or unequal. In the embodiment where the curved surface portions 22 are formed on all four sides, other features can refer to Figures 2 to 4 the settings of the illustrated embodiment, which will not be elaborated here.

[0065] Please refer to again Figure 2 , the adhesive layer 40 has adhesiveness and is very thin. Specifically, in this embodiment, the adhesive layer 40 is an optically transparent (OCA, Optically Clear Adhesive) glue. The adhesive layer 40 is attached to the inner surface provided with the glass substrate 20. Specifically, in this embodiment, the thickness of the adhesive layer 40 is 5 - 100 μm. More preferably, the thickness of the adhesive layer 40 is 5 - 20 μm.

[0066] The hardening layer 50 is formed on a surface of the adhesive layer 40 away from the glass substrate 20. As shown in Table 1, the evaluation results of the hardening layer 50 for Examples 1 - 7 are given.

[0067] Table 1

[0068] Hardened layer thickness Poor fracture Poor fitting of bubbles and wrinkles Example 1 0.5μm 22.5% 0.2% Example 2 1μm 13.4% 0.4% Example 3 2μm 5.1% 0.7% Example 4 3μm 1.7% 1.1% Example 5 5μm 0.9% 1.6% Example 6 10μm 0.3% 5.3% Example 7 20μm 0.1% 20.8%

[0069] The degree of folding is proportional to the thickness of the hardened layer, that is, the thinner the hardened layer is, the more likely it is that folding will occur when the hardened layer is bonded to the glass substrate.

[0070] Poor lamination of bubbles and wrinkles is proportional to the thickness of the hardened layer, that is, the thicker the hardened layer, the easier it is for bubbles or wrinkles to appear when the hardened layer is laminated to the glass substrate.

[0071] As shown in Table 1, in Examples 1 and 2, the hardened layer is too thin, and the hardened layer is closely attached to the glass substrate, and bubbles or wrinkles are not easy to appear, but folds are easy to appear. Therefore, when the hardened layer thickness in Example 1 is 0.5 μm, the fold defect rate is as high as 22.5%, while the lamination bubble and wrinkle defect rate is as low as 0.2%; when the hardened layer thickness in Example 2 is 1 μm, the fold defect rate reaches 13.4%, while the lamination bubble and wrinkle defect rate is 0.4%.

[0072] As shown in Table 1, when comparing Examples 1 to 7, it is confirmed that the hardened layer thickness of 2 to 10 μm shown in Examples 3 to 6 is more preferred. This preferred thickness can ensure that the folding defect is within an allowable range, while also ensuring fewer bonding bubbles and lower wrinkle defects.

[0073] When comparing Examples 1 to 6, it is confirmed that the thickness of the hardened layer shown in Examples 3 to 5 is greater than or equal to 2 μm and less than 5 μm, which is more preferred. This more preferred thickness can achieve the effects of lower folding defects, fewer bonding bubbles and lower wrinkles during the bonding process of the hardened layer and the glass substrate, thereby thinning the overall thickness of the cover glass laminate structure, thereby meeting the trend of thinning and lightweight electronic products with touch functions.

[0074] The UV texture layer 60 is UV transferred onto the hardening layer 50. Specifically, when forming the UV texture layer 60, UV glue can be coated on the hardening layer 50, and then the UV glue can be embossed by a template to give the UV glue a specific pattern, such as setting a specific pattern such as a brushed pattern, a CD pattern or a wavy pattern on the UV glue layer, and then a mask is applied to cure and clean the uncured UV glue, so that the UV texture layer 60 formed on the hardening layer 50 can be obtained.

[0075] The vapor deposition layer 70 is disposed on the UV texture layer 60, and the vapor deposition layer 70 may be, for example, a film layer showing a metallic color. With the pattern of the UV texture layer 60 as a foil, an appearance with different patterns and colors can be observed on one side of the outer surface 202 of the glass substrate 20, showing a metallic texture, thereby significantly improving the display effect of characters or icons and enhancing the user experience.

[0076] After the UV texture layer 60 is further provided with the vapor deposition layer 70 and other structures, since the vapor deposition layer 70 is non-transparent and the UV texture layer 60 is transparent, the patterns presented by the UV texture layer 60 and the vapor deposition layer 70 can still be observed on the outer surface 202 of the glass substrate 20 .

[0077] The ink layer 80 is disposed on the evaporation layer 70. Both the ink layer 80 and the evaporation layer 70 are opaque, so when observing from the outer surface 202 toward the inner surface 201, the scene on the other side of the glass substrate 20 blocked by the ink layer 80 and the evaporation layer 70 cannot be seen.

[0078] The cover glass laminate structure also includes a decorative layer 30, which is formed between the glass substrate 20 and the bonding layer 40. Specifically, the decorative layer 30 is formed by silk screen printing. Specifically, in the present embodiment, the decorative layer 30 is a black ring, which is a ring structure with a circular through hole. The black ring is directly formed on the glass substrate, which avoids the visual impact caused by the camera alignment error. In this way, the process can be simplified to reduce the alignment error, effectively improve the yield of the product, and at the same time, the visual impact caused by the camera alignment error is avoided, thereby improving the user experience. It can be understood that in other embodiments, the decorative layer 30 can be a character or icon, which is formed on the glass substrate by silk screen printing. Compared with the direct exposure, development and silk screen printing method to obtain characters or icons, there will be tooth edge jagged and other defects. The method provided by the present invention can effectively reduce the defects caused by the direct exposure and development of the decorative layer such as characters or icons, thereby effectively improving the yield of the product.

[0079] In some other embodiments, the glass substrate 20 is not limited to Figure 1-Figure 4 For example, Figure 5 and Figure 6 A glass substrate according to another embodiment is shown in FIG. 1 , which includes an inner surface 201 a , an outer surface 202 a spaced apart from the inner surface 201 a , and a side surface (not labeled) connecting the outer surface 202 a and the inner surface 201 a .

[0080] The distance between the inner surface 201a and the outer surface 202a is 0.2-1.0 mm, that is, the thickness of the glass substrate is 0.2-1.0 mm.

[0081] The inner surface 201a has a central axis 203a, and the inner surface 201a is symmetrically arranged along the central axis 203a. The outer surface 202a also has a central axis 204a, and the outer surface 202a is symmetrically arranged along the central axis 204a.

[0082] The inner surface 201a is bent toward the same side with the central axis 203a of the inner surface 201a as the center to form an inner curved surface of an arc, and the outer surface 202a is bent toward the same side with the central axis 204a of the outer surface 202a as the center to form an outer curved surface of an arc, the radius R of the inner curved surface and the outer curved surface is 50 to 1000 mm, and the height H of the glass substrate is 0.5 to 5 mm.

[0083] In some embodiments, the radii R of the inner curved surface and the outer curved surface are equal, that is, the thickness of the glass substrate is uniform everywhere, which can better eliminate stress concentration and improve the overall strength.

[0084] The height H of the glass substrate refers to the distance between the plane where the two parallel sides 205a and 206a of the inner surface 201a farthest from the central axis 203a thereof are located and the central axis 204a of the outer surface 202a.

[0085] In some embodiments, the angle between the two parallel sides 205a, 206a of the inner surface 201a and the line connecting the center of the arc, that is, the center angle of the arc corresponding to the inner surface 201a, is represented by C, where 60°<C<180°. The center angle C corresponding to the arc of the outer surface 202a also satisfies 60°<C<180°.

[0086] Figure 7 FIG. 1 is a glass substrate of another embodiment. Figure 8 and Fig. 9 The glass substrate includes an inner surface 201b, an outer surface 202b spaced apart from the inner surface 201b, and a side surface (not marked in the figure) connecting the outer surface 202b and the inner surface 201b.

[0087] The distance between the inner surface 201b and the outer surface 202b is 0.2-1.0 mm, that is, the thickness of the glass substrate is 0.2-1.0 mm.

[0088] The inner surface 201b has a center line W1 in the width direction, and the outer surface 202b also has a center line W2 in the width direction. The inner surface 201b is mirror-symmetrical along the center line W1. The outer surface 202b is mirror-symmetrical along the center line W2. The glass substrate is placed on a horizontal plane, and an orthographic projection is made on the glass substrate on the horizontal plane. The center line W1 of the inner surface 201b and the center line W2 of the outer surface 202b coincide with each other in the orthographic projection direction of the glass substrate.

[0089] Also refer to Fig.10 and Fig.11, the inner surface 201b has a center line L1 in the length direction, and the outer surface 202b also has a center line L2 in the length direction. The inner surface 201b is mirror-symmetrical along the center line L1. The outer surface 202b is mirror-symmetrical along the center line L2. The glass substrate is placed on a horizontal plane, and the glass substrate is orthographically projected on the horizontal plane. The center line L1 of the inner surface 201b and the center line L2 of the outer surface 202b coincide in the orthographic projection direction of the glass substrate. The orthographic projections of the center lines L1 and L2 are perpendicular to the orthographic projections of the center lines W1 and L2.

[0090] The inner surface 201b is curved toward the same side with the center line L1 in the length direction as the center, and the outer surface 202b is also curved toward the same side with the center line L2 in the length direction as the center. The arc radius of the center line L1 in the length direction of the inner surface 201b is 50 to 1000 mm, and the arc radius of the center line L2 in the length direction of the outer surface 202b is also 50 to 1000 mm. In the embodiment shown in the figure, the arc radii of the center lines L1 and L2 in the length direction of the inner surface 201b and the outer surface 202b are equal.

[0091] The inner surface 201b is also curved toward the same side with the center line W1 in the width direction as the center, and the outer surface 202b is also curved toward the same side with the center line W2 in the width direction as the center. The arc radius of the center line W1 in the width direction of the inner surface 201b is 50 to 1000 mm, and the arc radius of the center line W2 in the width direction of the outer surface 202b is also 50 to 1000 mm. The arc radii of the center lines W1 and W2 in the width direction of the inner surface 201b and the outer surface 202b are equal.

[0092] The height of the glass substrate is 0.5 to 5 mm. The height refers to the distance between the center point of the outer surface 202b (i.e., the intersection of the center line L2 in the length direction and the center line W2 in the width direction) and the plane formed by at least three lowest points of the inner surface 201. In the embodiment shown in the figure, the four corners of the inner surface 201b are located in the same plane, and the height is the distance between the plane where the four corners are located and the center point of the outer surface 202b.

[0093] In some embodiments, the thickness of the glass substrate is uniform at all locations, which can better eliminate stress concentration and improve overall strength.

[0094] In addition, the arc radius of the center lines W1 and W2 may be equal to or different from the arc radius of the center lines L1 and L2.

[0095] In some embodiments, the central angle corresponding to the arc of the center lines L1 and L2 of the inner surface 201b and the outer surface 202b in the length direction is C1, where 60°<C1<180°. The central angle corresponding to the arc of the center lines W1 and W2 of the inner surface 201b and the outer surface 202b in the width direction is C2, where 60°<C2<180°.

[0096] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0097] The cover glass laminate structure provided by the present invention has at least the following advantages:

[0098] The present invention adopts a cover glass laminate structure without a PET substrate, and the cover glass laminate structure includes a hardened layer with a thickness of 2 to 10 μm, which can ensure fewer laminating bubbles and fewer wrinkles. Furthermore, it is more preferred that the thickness of the hardened layer is greater than or equal to 2 μm and less than 5 μm. This more preferred thickness can achieve the effects of lower folding defects, fewer laminating bubbles and lower wrinkles during the laminating process between the hardened layer and the glass substrate, thereby reducing the overall thickness of the cover glass laminate structure, thereby meeting the trend of thinning and lightening of electronic products with touch functions.

[0099] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A cover glass laminate structure, It is characterized in that It consists of a glass substrate, a bonding layer and a hardening layer, a UV texture layer, a vapor deposition layer, an ink layer and a decorative layer; The glass substrate comprises an inner surface and an outer surface spaced apart from the inner surface; The adhesive layer is attached to the inner surface of the glass substrate; The hardening layer is formed on a surface of the bonding layer away from the glass substrate; Wherein, the thickness of the hardening layer is 2-10 μm; the thickness of the bonding layer is 5-100 μm; The hardening layer, UV texture layer, vapor deposition layer and ink layer are stacked in sequence; the vapor deposition layer is non-transparent, the vapor deposition layer is a film layer showing a metallic color, the UV texture layer is transparent, and the UV texture layer is transferred onto the hardening layer by UV; the decorative layer is formed between the glass substrate and the bonding layer; the decorative layer is a black ring, and the black ring is an annular structure with a circular through hole.

2. The cover glass laminate structure according to claim 1, It is characterized in that The thickness of the hardened layer is greater than or equal to 2 μm and less than 5 μm.

3. The cover glass laminate structure according to claim 1, It is characterized in that The thickness of the bonding layer is 5-20 μm.

4. The cover glass laminate structure according to claim 1, It is characterized in that The UV texture layer can form brushed texture, CD texture or wavy texture.

5. The cover glass laminate structure according to claim 1, It is characterized in that The decorative layer is formed by silk screen printing.

6. The cover glass laminate structure according to any one of claims 1 to 5, It is characterized in that The glass substrate has at least a partially curved surface.