Composite substrate, semiconductor device structure and preparation method thereof
By forming a protective layer and a semiconductor dielectric film layer on the growth substrate, and using an etching process to form a convex structure, the problem of low crystal quality of the GaN-based epitaxial layer is solved, and efficient LED epitaxial structure preparation and mass production are achieved.
Patent Information
- Application Number
- CN201711282031.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-12-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2037-12-07
AI Technical Summary
In the existing technology, the crystal quality of GaN-based epitaxial layers and LED epitaxial structures is not high, and the anisotropic performance indicators need to be improved, resulting in insufficient LED luminous efficiency and quality, making it difficult to achieve mass production.
A composite substrate preparation method is used, including forming an epitaxial buffer layer, a protective layer and a semiconductor dielectric film layer on the growth substrate, forming periodically spaced convex structures through photolithography and dry etching, and then using wet etching Remove the protective layer and pattern the protective layer to ensure the cleanliness of the epitaxial buffer layer and the connectivity of the semiconductor dielectric film layer, and improve the epitaxial growth conditions.
The crystal quality and light extraction rate of the epitaxial layer are improved, and the growth process window is expanded, making the composite substrate suitable for mass production and suitable for the preparation of semiconductor devices.
Smart Images

Figure CN108281525B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a composite substrate, a semiconductor device structure and a preparation method thereof. Background Art
[0002] As a new type of high-efficiency solid light source, semiconductor lighting has the advantages of long life, energy saving, environmental protection, safety, etc. Its application field is expanding rapidly. Especially in recent years, with the increase of research and development efforts and capital investment, the luminous efficiency and quality of LED have been greatly improved, and LED has been deeply applied.
[0003] After years of research and development, the LED industry has unanimously agreed that growth substrate technology is the core of GaN-based materials and devices. The current mainstream substrate technology routes are sapphire technology route, Si substrate technology route, SiC substrate technology route, GaN homogeneous substrate technology, and the latest breakthrough composite substrate technology route. Among the several technologies, the sapphire technology route is the most mature, and each of the several technology routes has its own advantages and disadvantages, and some still have technical difficulties. Their purpose is to improve the luminous efficiency and quality of LEDs.
[0004] The latest graphic substrates are as follows: 1. SiO2 is made on the surface of sapphire substrate or other conventional substrate surface. 2 1. Microscopic pattern of film structure; 2. Microscopic pattern of DBR film structure is made on the surface of sapphire substrate or other conventional substrate; 3. First, an epitaxial buffer layer is deposited on the growth substrate, and then SiO 2 、Si 3 N 4 Or the microscopic pattern of the DBR film structure. Both methods 1 and 2 have a common problem, that is, the subsequent epitaxial growth is difficult. If the growth is at a low temperature, SiO 2 Polycrystalline will be deposited on the surface of the film layer or DBR film layer, and the quality of the epitaxial crystal is poor. If grown at high temperature, GaN or polycrystalline cannot be deposited on the surface of the sapphire substrate, which makes the epitaxial growth process conditions extremely harsh and cannot be mass-produced. The third method is also somewhat difficult: First, SiO 2 The production of film structure micro-patterns, if wet etching of SiO 2 The size of the graphics will be limited and can only be made larger, not smaller, otherwise it cannot be mass-produced, not to mention nanoscale. If dry etching of SiO 2 The surface of the buffer layer will be contaminated by the etching gas, making subsequent epitaxial growth difficult or even impossible to deposit. The conditions are harsh and the quality of the epitaxial layer crystal is not improved much. The second is pure SiO 2 The film structure has limited light reflection effect and limited brightness improvement. All the above solutions cannot be mass-produced due to many problems.
[0005] To meet the requirements of higher LED applications, substrate technology needs to be improved and explored. Therefore, it is necessary to continuously explore substrate technology to effectively improve the quality of GaN-based epitaxial layers and LED epitaxial structure crystals and improve various LED performance indicators. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a composite substrate, a semiconductor device structure and a preparation method thereof, which are used to solve the problems of low crystal quality and poor anisotropic performance indicators in the prior art GaN-based epitaxial layer and LED epitaxial structure.
[0007] To achieve the above object and other related objects, the present invention provides a method for preparing a composite substrate, the method for preparing the composite substrate comprising the following steps:
[0008] 1) providing a growth substrate;
[0009] 2) forming an epitaxial buffer layer on the upper surface of the growth substrate;
[0010] 3) forming a protective layer on the upper surface of the epitaxial buffer layer;
[0011] 4) forming a semiconductor dielectric film layer on the upper surface of the protective layer;
[0012] 5) patterning the semiconductor dielectric film layer by photolithography and dry etching processes to form periodically spaced convex structures on the upper surface of the protective layer; a portion of the protective layer is exposed between the convex structures;
[0013] 6) Patterning the protective layer by a wet etching process to remove the exposed protective layer.
[0014] As a preferred solution of the method for preparing the composite substrate of the present invention, the protective layer includes a metal layer and / or a metal oxide layer.
[0015] As a preferred solution of the method for preparing the composite substrate of the present invention, the material of the metal layer includes nickel or titanium; the material of the metal oxide layer includes titanium oxide or indium tin oxide.
[0016] As a preferred solution of the method for preparing the composite substrate of the present invention, the semiconductor dielectric film layer includes at least one semiconductor dielectric layer.
[0017] As a preferred embodiment of the method for preparing the composite substrate of the present invention, the semiconductor dielectric film layer comprises SiO 2 Layer, Si 3 N 4 Layer, SiON xAt least one of a layer or a DBR layer.
[0018] As a preferred solution of the method for preparing the composite substrate of the present invention, the shape of the protrusion structure is cylindrical, square column, conical, bullet-shaped or strip-shaped.
[0019] The present invention also provides a composite substrate, comprising:
[0020] Growth substrate;
[0021] An epitaxial buffer layer, located on the upper surface of the growth substrate;
[0022] The protruding structures are distributed at periodic intervals on the upper surface of the epitaxial buffer layer; the protruding structures are semiconductor dielectric film layers;
[0023] The patterned protection layer is located between the protruding structure and the epitaxial buffer layer and is located directly below the protruding structure.
[0024] As a preferred solution of the composite substrate of the present invention, the protruding structure includes at least one semiconductor dielectric layer.
[0025] As a preferred embodiment of the method for preparing the composite substrate of the present invention, the semiconductor dielectric film layer comprises SiO 2 Layer, Si 3 N 4 Layer, SiON x At least one of a layer or a DBR layer.
[0026] As a preferred solution of the composite substrate of the present invention, the shape of the protrusion structure is cylindrical, square column, conical, bullet-shaped or strip-shaped.
[0027] As a preferred solution of the composite substrate of the present invention, the patterned protective layer includes a metal layer and / or a metal oxide layer.
[0028] As a preferred solution of the composite substrate of the present invention, the material of the metal layer includes nickel or titanium; the material of the metal oxide layer includes titanium oxide or indium tin oxide.
[0029] As a preferred solution of the composite substrate of the present invention, the thickness of the patterned protective layer is 10 angstroms to 500 angstroms.
[0030] The present invention also provides a method for preparing a semiconductor device structure, the method for preparing a semiconductor device structure comprising the following steps:
[0031] 1) preparing a composite substrate by using the preparation method described in any of the above schemes;
[0032] 2) forming an epitaxial transition layer on the surface of the composite substrate, wherein the epitaxial transition layer fills the gaps between the protruding structures and completely covers the protruding structures;
[0033] 3) forming an N-type epitaxial layer on the surface of the epitaxial transition layer;
[0034] 4) forming a quantum well layer on the surface of the N-type epitaxial layer;
[0035] 5) Forming a P-type epitaxial layer on the surface of the quantum well layer.
[0036] As a preferred solution of the method for preparing the semiconductor device structure of the present invention, after step 5), it also includes the steps of forming an N electrode on the surface of the N-type epitaxial layer and forming a P electrode on the surface of the P-type epitaxial layer.
[0037] As a preferred solution of the method for preparing the semiconductor device structure of the present invention, after step 5), it also includes the steps of forming a P electrode on the surface of the P-type epitaxial layer and forming an N electrode on the surface of the growth substrate away from the epitaxial buffer layer.
[0038] The present invention also provides a semiconductor device structure, the semiconductor device structure comprising:
[0039] A composite substrate as described in any of the above schemes;
[0040] An epitaxial transition layer fills the gaps between the protruding structures and completely covers the protruding structures;
[0041] An N-type epitaxial layer, located on the surface of the epitaxial transition layer;
[0042] A quantum well layer, located on the surface of the N-type epitaxial layer;
[0043] A P-type epitaxial layer and a surface of the quantum well layer.
[0044] As a preferred solution of the semiconductor device structure of the present invention, the semiconductor device structure further includes:
[0045] An N electrode, located on the surface of the N-type epitaxial layer;
[0046] The P electrode is located on the surface of the P-type epitaxial layer.
[0047] As a preferred solution of the semiconductor device structure of the present invention, the semiconductor device structure further includes:
[0048] A P electrode, located on the surface of the P-type epitaxial layer;
[0049] The N electrode is located on a surface of the growth substrate away from the epitaxial buffer layer.
[0050] As described above, the composite substrate, semiconductor device structure and preparation method thereof of the present invention have the following beneficial effects:
[0051] The preparation method of the composite substrate of the present invention forms a protective layer on the surface of the epitaxial buffer layer first, and then forms a semiconductor dielectric film layer on the surface of the protective layer. In the process of etching the semiconductor dielectric film layer by a dry etching process to form a protruding structure, the protective layer plays a role in protecting the epitaxial buffer layer, so that the epitaxial buffer layer will not be contaminated by etching gas or polymer in the dry etching process, making it easier to epitaxially grow the epitaxial layer on the surface of the epitaxial buffer layer again, and the growth process window is larger, which can be mass-produced by process technology; at the same time, the protective layer also plays a role in connecting the epitaxial buffer layer with the semiconductor dielectric film layer, so that when the composite substrate is used for the preparation of semiconductor device structure, it can resist the change of stress during the temperature rise process of epitaxial growth; because the protective layer is designed to be very thin, it is not easy to be etched during wet etching, so that the accuracy of the pattern can be well controlled.
[0052] The raised structures distributed in a periodic array in the composite substrate of the present invention and including at least one semiconductor dielectric layer can improve the crystal quality of the epitaxial layer laterally grown on the surface of the composite substrate; at the same time, since the raised structure is a semiconductor dielectric film layer, each layer in the raised structure has a large reflectivity difference with the GaN layer in the semiconductor device subsequently formed on the surface of the composite substrate, and the reflective effect of the raised structure is better, which can improve the light extraction rate of the semiconductor device subsequently formed on the surface of the composite substrate.
[0053] The innovative design of the composite substrate preparation process of the present invention enables the composite substrate of the present invention to not only exert its technical performance advantages but also be mass-produced and promoted on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 Shown is a flow chart of a method for preparing a composite substrate provided in Embodiment 1 of the present invention.
[0055] Figures 2 to 11 The structure schematic diagram of each step of the method for preparing a composite substrate provided in the first embodiment of the present invention is shown, wherein: Figures 9 to 11 The structure diagram of the composite substrate provided by the present invention is shown, wherein: Fig. 9 is a top view, Fig.10 and Fig.11 A cross-sectional view.
[0056] Fig.12 Shown is a flow chart of a method for preparing a semiconductor device structure provided in Embodiment 3 of the present invention.
[0057] Figures 13 to 18It is a schematic diagram showing the structure of each step of the method for preparing a semiconductor device structure provided in the third embodiment of the present invention, wherein: Fig.17 and Fig.18 Shown is a schematic cross-sectional structure diagram of a semiconductor device structure provided by the present invention.
[0058] Component number description
[0059] 10 Growth substrate
[0060] 11 Epitaxial buffer layer
[0061] 12 protection layers
[0062] 121 Graphical protective layer
[0063] 13Semiconductor dielectric film layer
[0064] 131SiO 2 layer
[0065] 132Si 3 N 4 layer
[0066] 133 Raised structure
[0067] 14 Epitaxial transition layer
[0068] 15N epitaxial layer
[0069] 16 quantum well layers
[0070] 17P epitaxial layer
[0071] 18N Electrode
[0072] 19P electrode DETAILED DESCRIPTION
[0073] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0074] See also Figures 1 to 18 It should be noted that the illustrations provided in this embodiment are only schematic illustrations of the basic concept of the present invention. Although the illustrations only show components related to the present invention and are not drawn according to the number, shape and size of components in actual implementation, the type, quantity and proportion of each component in actual implementation may be changed arbitrarily, and the component layout may also be more complicated.
[0075] Embodiment 1
[0076] See also Figure 1 The present invention provides a method for preparing a composite substrate, the method for preparing the composite substrate comprising the following steps:
[0077] 1) providing a growth substrate;
[0078] 2) forming an epitaxial buffer layer on the upper surface of the growth substrate;
[0079] 3) forming a protective layer on the upper surface of the epitaxial buffer layer;
[0080] 4) forming a semiconductor dielectric film layer on the upper surface of the protective layer;
[0081] 5) patterning the semiconductor dielectric film layer by photolithography and dry etching processes to form periodically spaced convex structures on the upper surface of the protective layer; a portion of the protective layer is exposed between the convex structures;
[0082] 6) Patterning the protective layer by a wet etching process to remove the exposed protective layer.
[0083] In step 1), refer to Figure 1 The S1 step in Figure 2 , providing a growth substrate 10.
[0084] As an example, the growth substrate 10 can be selected according to actual needs. Preferably, the growth substrate 10 can be Al 2 O 3 substrate, SiC substrate, Si substrate, ZnO substrate or GaN substrate.
[0085] In step 2), refer to Figure 1 The S2 step in Figure 3 , an epitaxial buffer layer 11 is formed on the surface of the growth substrate 10 .
[0086] As an example, the epitaxial buffer layer 11 may be a nitride buffer layer. Preferably, in this embodiment, the epitaxial buffer layer 11 may be an Al x Ga 1-x The N layer may be a BN layer, wherein 0≤x≤0.5; or the AlN layer may be a (0001) crystal orientation.
[0087] As an example, the epitaxial buffer layer 11 may be formed on the surface of the growth substrate 10 by using a MOCVD (metal organic chemical vapor deposition), HVPE (hydride vapor phase epitaxy) or PVD (physical vapor deposition) process.
[0088] As an example, the thickness of the epitaxial buffer layer 11 can be set according to actual needs. Preferably, in this embodiment, the thickness of the epitaxial buffer layer 11 is 50 angstroms to 600 angstroms.
[0089] In step 3), refer to Figure 1 The S3 steps in Figure 4 A protective layer 12 is formed on the upper surface of the epitaxial buffer layer 11 .
[0090] As an example, the protective layer 12 can be formed on the upper surface of the epitaxial buffer layer 11 by evaporation or other processes; the protective layer 12 can include a metal layer and / or a metal oxide layer, that is, the protective layer 12 can be a metal layer, or at least two metal layers of different materials, or a metal oxide layer, or at least two metal oxide layers of different materials, or a stacked structure consisting of at least one metal layer and at least one metal oxide layer. Specifically, the material of the metal layer includes nickel (Ni) or titanium (Ti); the material of the metal oxide layer includes titanium oxide (TiOx) or indium tin oxide (ITO). In one example, the protective layer 12 includes a titanium oxide layer and an indium tin oxide layer.
[0091] As an example, the thickness of the protective layer 12 can be set according to actual needs. Preferably, in this embodiment, the thickness of the protective layer 12 can be 10 angstroms to 500 angstroms. If the thickness of the protective layer 12 is too small, such as less than 10 angstroms, the protective effect it plays will be very limited. If the thickness of the protective layer 12 is too large, such as greater than 500 angstroms, it is easy to cause undercutting, thereby affecting the performance of the device. In the present invention, the thickness of the protective layer 12 is set to 10 angstroms to 500 angstroms, which can ensure the protective effect of the protective layer 12 and is not easy to be undercut during subsequent wet etching, so that the accuracy of the pattern can be well controlled.
[0092] In step 4), refer to Figure 1 Step S4 in Figure 5 , a semiconductor dielectric film layer 13 is formed on the upper surface of the protective layer 12 .
[0093] As an example, at least one semiconductor dielectric layer is deposited on the upper surface of the protective layer 12 as the semiconductor dielectric film layer 13 by using processes such as plasma enhanced chemical vapor deposition (PECVD), PVD or electron beam evaporation. When the semiconductor dielectric film layer 13 includes at least two semiconductor dielectric layers, at least two semiconductor dielectric layers can be deposited sequentially or alternately to form the semiconductor dielectric film layer 13. The materials of the adjacent semiconductor dielectric layers are different, and the reflectivity of the semiconductor dielectric layer is significantly different from the reflectivity of GaN.
[0094] As an example, the semiconductor dielectric film layer 13 includes SiO 2 Layer, Si 3 N 4 、SiON x At least one of a layer or a DBR layer (the DBR layer is a film layer composed of titanium dioxide and silicon oxide alternately stacked). Specifically, the semiconductor dielectric film layer 13 may include SiO 2 Layer, Si 3 N 4 、SiON x The single-layer structure of the layer or DBR layer may also include SiO 2 Layer and Si 3 N 4 The two-layer structure may also include SiO 2 Layer and Si 3 N 4 The multilayer structure may also include SiO 2 Layer, Si 3 N 4 and SiON x The three-layer structure may also include SiO 2 Layer, Si 3 N 4 、SiON x The multilayer structure of the layer and the DBR layer may also include SiO 2 Layer, Si 3 N 4 、SiON x The multilayer structure of the layer and the DBR layer. Figure 5 The semiconductor dielectric film layer 13 includes SiO 2 Layer 131 and Si 3 N 4 A two-layer structure of layer 132 is exemplified.
[0095] In step 5), refer to Figure 1 Step S5 in Figures 6 to 8 ,in, Figure 7 and Figure 8 for Figure 6 , the semiconductor dielectric film layer 13 is patterned by photolithography and dry etching processes to form periodically spaced convex structures 133 on the upper surface of the protective layer 12; a portion of the protective layer 12 is exposed between the convex structures 133.
[0096] As an example, the protrusion structures 133 are distributed in a periodic hexagonal pattern on the upper surface of the protection layer 12 , or may be distributed in an array.
[0097] As an example, the shape of the protrusion structure 133 is cylindrical, square, conical, bar or bullet-shaped. Figure 7 FIG. 1 is a schematic diagram of a cross-sectional structure in which the protruding structure 133 is in the shape of a bullet head. Figure 8 FIG. 1 is a schematic diagram of a cross-sectional structure in which the protrusion structure 133 is in a cylindrical or square column shape.
[0098] As an example, the maximum lateral dimension of the protruding structure 133 is 0.1 μm to 10 μm, that is, the dimension of the bottom of the protruding structure 133 is 0.1 μm to 10 μm; the height of the protruding structure 133 is 0.2 μm to 3 μm, that is, the thickness of the semiconductor dielectric film layer 13 formed in step 4) is 0.2 μm to 3 μm; the minimum spacing between adjacent protruding structures 133 is 0.1 μm to 5 μm, that is, the spacing between the bottoms of adjacent protruding structures 133 is 0.1 μm to 5 μm.
[0099] In step 5), since the protective layer 12 is formed under the semiconductor dielectric film layer 13, in the process of etching the semiconductor dielectric film layer 13 by a dry etching process to form the protruding structure 133, the protective layer 12 plays a role in protecting the epitaxial buffer layer 11, so that the epitaxial buffer layer 11 will not be contaminated by the etching gas or polymer in the dry etching process, making it easier to epitaxially grow an epitaxial layer on the surface of the epitaxial buffer layer 11 again, and the growth process window is larger, which can be mass-produced by process technology; at the same time, the protective layer 12 also plays a role in connecting the epitaxial buffer layer 11 with the semiconductor dielectric film layer 13 (the protruding structure 133 after etching), so that when the composite substrate is used for the preparation of semiconductor device structure, it can resist the change of stress during the heating process of epitaxial growth.
[0100] The raised structures 133 distributed in a periodic array and including at least one semiconductor dielectric layer in the composite substrate of the present invention can improve the crystal quality of the epitaxial layer grown laterally formed on the surface of the composite substrate; at the same time, since the raised structures 133 are semiconductor dielectric film layers, each layer in the raised structures 133 and the GaN layer in the semiconductor device subsequently formed on the surface of the composite substrate have a large reflectivity difference, and the reflective effect of the raised structures 133 is better, which can improve the light extraction rate of the semiconductor device subsequently formed on the surface of the composite substrate.
[0101] In step 6), refer to Figure 1 Step S6 in Figures 9 to 11 ,in, Fig.10 and Fig.11 for Fig. 9, the protective layer 12 is patterned by a wet etching process to remove the exposed protective layer 12, and the protective layer 12 retained directly below the protruding structure 133 is the patterned protective layer 121.
[0102] As an example, an existing wet etching solution that can remove the protective layer 12 but cannot remove other structures around the protective layer 12 can be used to remove the exposed protective layer 12 (i.e., the protective layer 12 located between adjacent protruding structures 133). After removing the exposed protective layer 12, the epitaxial buffer layer 11 located between the protruding structures 133 is exposed. It should be noted that in step 6), all the protective layers 12 located between the protruding structures 133 and the periphery of the protruding structures 133 are completely removed, so that the epitaxial buffer layer 11 except for the protruding structures 133 is exposed.
[0103] Embodiment 2
[0104] Please continue reading Fig. 9 and Fig.11 The present invention also provides a composite substrate, which can be prepared by the preparation method described in Example 1, and includes: a growth substrate 10; an epitaxial buffer layer 11, wherein the epitaxial buffer layer 11 is located on the upper surface of the growth substrate 10; a protruding structure 133, wherein the protruding structure 133 is periodically distributed on the upper surface of the epitaxial buffer layer 11; the protruding structure 133 is a semiconductor dielectric film layer; and a patterned protective layer 121, wherein the patterned protective layer 121 is located between the protruding structure 133 and the epitaxial buffer layer 11, and is located directly below the protruding structure 133.
[0105] As an example, the growth substrate 10 may be Al 2 O 3 substrate, SiC substrate, Si substrate, ZnO substrate or GaN substrate.
[0106] As an example, the epitaxial buffer layer 11 may be Al x Ga 1-x The N layer may be a BN layer, wherein 0≤x≤0.5; or the AlN layer may be a (0001) crystal orientation.
[0107] As an example, the thickness of the epitaxial buffer layer 11 can be set according to actual needs. Preferably, in this embodiment, the thickness of the epitaxial buffer layer 11 is 50 angstroms to 600 angstroms.
[0108] As an example, the patterned protective layer 121 may include a metal layer and / or a metal oxide layer, that is, the patterned protective layer 121 may be a metal layer, or at least two metal layers of different materials, or a metal oxide layer, or at least two metal oxide layers of different materials, or a laminated structure consisting of at least one metal layer and at least one metal oxide layer. Specifically, the material of the metal layer includes nickel (Ni) or titanium (Ti); the material of the metal oxide layer includes titanium oxide (TiOx) or indium tin oxide (ITO). In one example, the patterned protective layer 121 includes a titanium oxide layer and an indium tin oxide layer.
[0109] As an example, the patterned protection layer 121 is obtained by etching the protection layer 12 described in the first embodiment.
[0110] As an example, the thickness of the protective layer 12 can be set according to actual needs. Preferably, in this embodiment, the thickness of the protective layer 12 can be 10 angstroms to 500 angstroms.
[0111] As an example, the protruding structure 133 includes at least one semiconductor dielectric layer. When the protruding structure 133 includes at least two semiconductor dielectric layers, the materials of adjacent semiconductor dielectric layers are different, and the reflectivity of the semiconductor dielectric layer is significantly different from that of GaN.
[0112] As an example, the protrusion structure 133 includes SiO 2 Layer, Si 3 N 4 Layer, SiON x Specifically, the protrusion structure 133 may include SiO 2 Layer, Si 3 N 4 Layer, SiON x The single-layer structure of the layer or DBR layer may also include SiO 2 Layer and Si 3 N 4 The two-layer structure may also include SiO 2 Layer and Si 3 N 4 The multilayer structure may also include SiO 2 Layer, Si 3 N 4 Layer and SiON x The three-layer structure may also include SiO 2 Layer, Si 3 N 4 Layer, SiONx The multilayer structure of the layer and the DBR layer may also include SiO 2 Layer, Si 3 N 4 Layer, SiON x The multilayer structure of the layer and the DBR layer. Fig.10 and Fig.11 The protruding structure 133 includes SiO 2 Layer 131, Si 3 N 4 A two-layer structure of layer 132 is exemplified.
[0113] As an example, the protrusion structures 133 are distributed in a periodic hexagonal pattern on the surface of the epitaxial buffer layer 11 , or may be distributed in an array pattern.
[0114] As an example, the shape of the protrusion structure 133 is cylindrical, square column, conical, bar, bullet head or bar. Fig.10 FIG. 1 is a schematic diagram of a cross-sectional structure in which the protruding structure 133 is in the shape of a bullet head. Fig.11 FIG. 1 is a schematic diagram of a cross-sectional structure in which the protrusion structure 133 is in a cylindrical or square column shape.
[0115] As an example, the maximum lateral dimension of the protruding structure 133 is 0.1 μm to 10 μm, that is, the dimension of the bottom of the protruding structure 133 is 0.1 μm to 10 μm; the height of the protruding structure 133 is 0.2 μm to 3 μm, that is, the thickness of the protruding structure 133 is 0.2 μm to 3 μm; the minimum spacing between adjacent protruding structures 133 is 0.1 μm to 5 μm, that is, the spacing between the bottoms of adjacent protruding structures 133 is 0.1 μm to 5 μm.
[0116] The patterned protective layer 121 of the present invention is obtained by etching the protective layer 12 formed under the semiconductor dielectric film layer 13. In the process of etching the semiconductor dielectric film layer 13 by a dry etching process to form the protruding structure 133, the protective layer 12 plays a role in protecting the epitaxial buffer layer 11, so that the epitaxial buffer layer 11 will not be contaminated by the etching gas or polymer in the dry etching process, making it easier to epitaxially grow an epitaxial layer on the surface of the epitaxial buffer layer 11 again, and the growth process window is larger, which can be mass-produced by process technology; at the same time, the protective layer 12 also plays a role in connecting the epitaxial buffer layer 11 with the semiconductor dielectric film layer 13 (the protruding structure 133 after etching), so that when the composite substrate is used for the preparation of semiconductor device structure, it can resist the change of stress during the temperature rise process of epitaxial growth.
[0117] The raised structures 133 distributed in a periodic array and including at least one semiconductor dielectric layer in the composite substrate of the present invention can improve the crystal quality of the epitaxial layer grown laterally formed on the surface of the composite substrate; at the same time, since the raised structures 133 are semiconductor dielectric film layers, each layer in the raised structures 133 and the GaN layer in the semiconductor device subsequently formed on the surface of the composite substrate have a large reflectivity difference, and the reflective effect of the raised structures 133 is better, which can improve the light extraction rate of the semiconductor device subsequently formed on the surface of the composite substrate.
[0118] Embodiment 3
[0119] See also Fig.12 The present invention also provides a method for preparing a semiconductor device structure, the method for preparing a semiconductor device structure comprising the following steps:
[0120] 1) preparing a composite substrate by the preparation method described in Example 1;
[0121] 2) forming an epitaxial transition layer on the surface of the composite substrate, wherein the epitaxial transition layer fills the gaps between the protruding structures and completely covers the protruding structures;
[0122] 3) forming an N-type epitaxial layer on the surface of the epitaxial transition layer;
[0123] 4) forming a quantum well layer on the surface of the N-type epitaxial layer;
[0124] 5) Forming a P-type epitaxial layer on the surface of the quantum well layer.
[0125] In step 1), refer to Fig.12 In step S1 of the embodiment, the composite substrate is prepared by the preparation method described in the first embodiment.
[0126] The specific method for preparing the composite substrate can be found in Example 1 and will not be described again here.
[0127] In step 2), refer to Fig.12 The S2 step in Fig.13 , an epitaxial transition layer 14 is formed on the surface of the composite substrate, and the epitaxial transition layer 14 fills the gaps between the protruding structures 133 and completely covers the protruding structures 133 .
[0128] As an example, the epitaxial transition layer 14 is formed on the exposed upper surface of the epitaxial buffer layer 11 by using a MOCVD or HVPE process.
[0129] As an example, the thickness of the epitaxial transition layer 14 can be set according to actual needs. Preferably, in this embodiment, the thickness of the epitaxial transition layer 14 can be 1 μm to 10 μm.
[0130] In one example, the epitaxial transition layer 14 is a single-layer structure, and the epitaxial transition layer 14 can be a GaN layer, an AlGaN layer, an AlN layer, an InGaN layer, an AlInGaN layer, a Si-doped N-type semiconductor material layer, or a Mg-doped P-type semiconductor material layer.
[0131] In another example, the epitaxial transition layer 14 is a two-layer or multi-layer stacked structure, and the epitaxial transition layer 14 can be a stacked structure of at least two of a GaN layer, an AlGaN layer, an AlN layer, an InGaN layer, an AlInGaN layer, a Si-doped N-type semiconductor material layer, or a Mg-doped P-type semiconductor material layer.
[0132] It should be noted that, in this embodiment, the shape of the protruding structure 133 is a bullet shape as an example, and the process methods and structures corresponding to the protruding structures 133 of other shapes are the same as those in this embodiment.
[0133] In step 3), refer to Fig.12 The S3 steps in Fig.14 , an N-type epitaxial layer 15 is formed on the surface of the epitaxial transition layer 14 .
[0134] As an example, the N-type epitaxial layer 15 may be formed on the surface of the epitaxial transition layer 14 by using a MOCVD process.
[0135] In step 4), refer to Fig.12 Step S4 in Fig.15 , a quantum well layer 16 is formed on the surface of the N-type epitaxial layer 15 .
[0136] As an example, the quantum well layer 16 may be formed on the surface of the N-type epitaxial layer 15 by using a MOCVD process.
[0137] In step 5), refer to Fig.12 Step S5 in Fig.16 , a P-type epitaxial layer 17 is formed on the surface of the quantum well layer 16 .
[0138] As an example, the P-type epitaxial layer 17 may be formed on the surface of the quantum well layer 16 by using a MOCVD process.
[0139] In one example, see Fig.17 After step 5), the method further includes forming an N electrode 18 on the surface of the N-type epitaxial layer 15 and forming a P electrode 19 on the surface of the P-type epitaxial layer 17.
[0140] As an example, when forming the N-electrode 18 on the surface of the N-type epitaxial layer 15, a photolithography process is first used to remove part of the quantum well layer 16 and part of the P-type epitaxial layer 17 to expose the N-type epitaxial layer 15 to form a step structure, and then the N-electrode is formed on the surface of the N-type epitaxial layer 15. Of course, after the N-electrode 15 is exposed to form a step structure, the N-electrode 18 can be formed on the surface of the N-type epitaxial layer 15 and the P-electrode 16 can be formed on the surface of the P-electrolyte 17 at the same time.
[0141] In another example, see Fig.18 After step 5), the method further includes forming a P electrode 19 on the surface of the P-type epitaxial layer 17 and forming an N electrode 18 on the surface of the growth substrate 10 away from the epitaxial buffer layer 11.
[0142] Embodiment 4
[0143] Please continue reading Fig.17 and Fig.18 The present invention also provides a semiconductor device structure, which can be prepared by the preparation method in Example 3, and the semiconductor device structure includes: the composite substrate as described in Example 2; an epitaxial transition layer 14, wherein the epitaxial transition layer 14 fills the gaps between the protruding structures 133 and completely covers the protruding structures 133; an N-type epitaxial layer 15, wherein the N-type epitaxial layer 15 is located on the surface of the epitaxial transition layer 14; a quantum well layer 16, wherein the quantum well layer 16 is located on the surface of the N-type epitaxial layer 15; and a P-type epitaxial layer 17, wherein the P-type epitaxial layer 17 and the surface of the quantum well layer 16.
[0144] As an example, the thickness of the epitaxial transition layer 14 can be set according to actual needs. Preferably, in this embodiment, the thickness of the epitaxial transition layer 14 can be 1 μm to 10 μm.
[0145] In one example, the epitaxial transition layer 14 is a single-layer structure, and the epitaxial transition layer 14 can be a GaN layer, an AlGaN layer, an AlN layer, an InGaN layer, an AlInGaN layer, a Si-doped N-type semiconductor material layer, or a Mg-doped P-type semiconductor material layer.
[0146] In another example, the epitaxial transition layer 14 is a two-layer or multi-layer stacked structure, and the epitaxial transition layer 14 can be a stacked structure of at least two of a GaN layer, an AlGaN layer, an AlN layer, an InGaN layer, an AlInGaN layer, a Si-doped N-type semiconductor material layer, or a Mg-doped P-type semiconductor material layer.
[0147] It should be noted that, in this embodiment, the shape of the protruding structure 133 is also a bullet shape as an example.
[0148] In one example, if Fig.17 As shown, the semiconductor device structure further includes: an N-electrode 18 , which is located on the surface of the N-type epitaxial layer 15 ; and a P-electrode 19 , which is located on the surface of the P-type epitaxial layer 17 .
[0149] In another example, if Fig.18 As shown, the semiconductor device structure further includes: a P electrode 19 , which is located on the surface of the P-type epitaxial layer 17 ; and an N electrode 18 , which is located on the surface of the growth substrate 10 away from the epitaxial buffer layer 11 .
[0150] In summary, the present invention provides a composite substrate, a semiconductor device structure and a method for preparing the same. The method for preparing the composite substrate comprises the following steps: 1) providing a growth substrate; 2) forming an epitaxial buffer layer on the upper surface of the growth substrate; 3) forming a protective layer on the upper surface of the epitaxial buffer layer; 4) forming a semiconductor dielectric film layer on the upper surface of the protective layer; 5) patterning the semiconductor dielectric film layer using photolithography and dry etching processes to form periodically spaced raised structures on the upper surface of the protective layer; a portion of the protective layer is exposed between the raised structures; and 6) patterning the protective layer using a wet etching process to remove the exposed protective layer. The preparation method of the composite substrate of the present invention comprises the following steps: firstly forming a protective layer on the surface of the epitaxial buffer layer, and then forming a semiconductor dielectric film layer on the surface of the protective layer. In the process of etching the semiconductor dielectric film layer by a dry etching process to form a convex structure, the protective layer plays a role in protecting the epitaxial buffer layer, so that the epitaxial buffer layer will not be contaminated by etching gas or polymer in the dry etching process, so that it is easier to epitaxially grow an epitaxial layer on the surface of the epitaxial buffer layer again, the growth process window is larger, and process-based mass production is possible; at the same time, the protective layer also plays a role in connecting the epitaxial buffer layer with the semiconductor dielectric film layer, so that when the composite substrate is used When preparing the semiconductor device structure, it can resist the change of stress during the temperature rise process of epitaxial growth; the convex structure distributed in a periodic array in the composite substrate of the present invention and including at least one semiconductor dielectric layer can make the crystal quality of the epitaxial layer formed on the surface of the composite substrate laterally grown better; at the same time, because the convex structure is a semiconductor dielectric film layer, each layer in the convex structure and the GaN layer in the semiconductor device subsequently formed on the surface of the composite substrate have a large reflectivity difference, the reflective effect of the convex structure is better, and the light extraction rate of the semiconductor device subsequently formed on the surface of the composite substrate can be improved.
[0151] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a composite substrate, characterized in that: The method for preparing the composite substrate comprises the following steps: 1) providing a growth substrate; 2) forming an epitaxial buffer layer on the upper surface of the growth substrate; 3) forming a protective layer on the upper surface of the epitaxial buffer layer; 4) forming a semiconductor dielectric film layer on the upper surface of the protective layer; 5) patterning the semiconductor dielectric film layer by photolithography and dry etching processes to form periodically spaced convex structures on the upper surface of the protective layer; a portion of the protective layer is exposed between the convex structures; 6) Patterning the protective layer by a wet etching process to remove the exposed protective layer, retaining the protective layer directly below the protruding structure to form a patterned protective layer, wherein the patterned protective layer is a metal layer, the material of the metal layer is nickel or titanium, the thickness of the metal layer ranges from 10 angstroms to 500 angstroms, and is used to connect the epitaxial buffer layer and the protruding structure.
2. The method for preparing a composite substrate according to claim 1, characterized in that: The semiconductor dielectric film layer includes at least one semiconductor dielectric layer.
3. The method for preparing a composite substrate according to claim 2, characterized in that: The semiconductor dielectric film layer includes a SiO2 layer, a Si3N4 layer, a SiON x Or at least one of the DBR layers.
4. The method for preparing a composite substrate according to claim 1, characterized in that: The shape of the protruding structure is cylindrical, square column, conical or bullet-shaped.
5. A composite substrate, characterized in that: The composite substrate comprises: Growth substrate; An epitaxial buffer layer, located on the upper surface of the growth substrate; The protruding structures are distributed at periodic intervals on the upper surface of the epitaxial buffer layer; the protruding structures are semiconductor dielectric film layers; A patterned protective layer formed by a wet etching process is located between the protruding structure and the epitaxial buffer layer and directly below the protruding structure. The patterned protective layer is a metal layer. The material of the metal layer is nickel or titanium. The thickness of the metal layer ranges from 10 angstroms to 500 angstroms and is used to connect the epitaxial buffer layer and the protruding structure.
6. The composite substrate according to claim 5, characterized in that: The protruding structure includes at least one semiconductor dielectric layer.
7. The composite substrate according to claim 6, characterized in that: The semiconductor dielectric film layer includes a SiO2 layer, a Si3N4 layer, a SiON x At least one of a layer or a DBR layer.
8. The composite substrate according to claim 5, characterized in that: The shape of the protruding structure is cylindrical, square column, conical or bullet-shaped.
9. A method for preparing a semiconductor device structure, characterized in that: The method for preparing the semiconductor device structure comprises the following steps: 1) preparing a composite substrate by the preparation method according to any one of claims 1 to 4; 2) forming an epitaxial transition layer on the surface of the composite substrate, wherein the epitaxial transition layer fills the gaps between the protruding structures and completely covers the protruding structures; 3) forming an N-type epitaxial layer on the surface of the epitaxial transition layer; 4) forming a quantum well layer on the surface of the N-type epitaxial layer; 5) Forming a P-type epitaxial layer on the surface of the quantum well layer.
10. The method for preparing a semiconductor device structure according to claim 9, characterized in that: After step 5), the method further includes forming an N electrode on the surface of the N-type epitaxial layer and forming a P electrode on the surface of the P-type epitaxial layer.
11. The method for preparing a semiconductor device structure according to claim 9, characterized in that: After step 5), the method further includes forming a P electrode on the surface of the P-type epitaxial layer and forming an N electrode on the surface of the growth substrate away from the epitaxial buffer layer.
12. A semiconductor device structure, characterized in that: The semiconductor device structure comprises: The composite substrate according to any one of claims 5 to 8; An epitaxial transition layer fills the gaps between the protruding structures and completely covers the protruding structures; An N-type epitaxial layer, located on the surface of the epitaxial transition layer; A quantum well layer, located on the surface of the N-type epitaxial layer; A P-type epitaxial layer and a surface of the quantum well layer.
13. The semiconductor device structure according to claim 12, characterized in that: The semiconductor device structure further includes: An N electrode, located on the surface of the N-type epitaxial layer; The P electrode is located on the surface of the P-type epitaxial layer.
14. The semiconductor device structure according to claim 12, characterized in that: The semiconductor device structure further includes: A P electrode, located on the surface of the P-type epitaxial layer; The N electrode is located on a surface of the growth substrate away from the epitaxial buffer layer.
Citation Information
Patent Citations
Method for eliminating epitaxial layer growth mismatch by using low melting point metal
CN104409336A
Composite substrate, semiconductor device structure and fabrication method of composite substrate
CN106784217A
Composite substrate and semiconductor device structure
CN207651512U
Semiconductor light-emitting device and method of fabricating the same
US20090090931A1
Composite substrate of gallium nitride and metal oxide
US20140054595A1