Method for preparing active carbon with developed mesopores by using coal
A kind of activated carbon, developed technology, applied in the field of coal-based activated carbon preparation, can solve the problem of low mesoporosity, achieve the effect of increasing mesoporosity, improving production efficiency, and reducing costs
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2018-08-24
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention belongs to the field of coal-based activated carbon preparation, in particular to a method for preparing activated carbon with well-developed mesopores by using coal. Background technique
[0002] Because activated carbon has a highly developed pore structure and a large specific surface area, its applications range from decolorization and deodorization of food and medicine, gas masks, to large-scale use in solvent refining and recovery, advanced water treatment, flue gas Purification, blood purification, etc., put forward new and higher requirements for the adsorption performance of activated carbon.
[0003] Activated carbon is divided according to its form, including shaped activated carbon and powdered activated carbon. Compared with shaped activated carbon, powdered activated carbon has greater adsorption (iodine value and / or methylene blue value), but due to its powdery form, it is limited. application field.
[0004] China is ric...
Examples
Embodiment 1
[0038] Coal A, which accounts for 60wt% of the total amount of raw coal, and 40wt% coal B are ground into pulverized coal less than 200 mesh in a mill, and sent to a briquetting machine with a working pressure of 26MP for briquetting. After primary crushing and secondary Screening after crushing;
[0039] Qualified pellets (1mm ~ 8mm) are subjected to oxidation treatment and carbonization treatment in sequence, and the oxidation treatment conditions are: oxidize the pellets for 3 hours at 230-250°C with air as the oxidant in an electrically heated external heating converter Treatment; the carbonization treatment conditions are as follows: carbonize the material for 2.5 hours at 500-550°C in an electric heating external heating converter, and control the oxygen concentration in the furnace atmosphere below 5vol%.
[0040] After cooling, the carbonized material obtained is soaked in 5% sodium nitrate solution for 2 hours, dried (the nitrate content is about 0.6%), and then sent ...
Embodiment 2
[0042] Coal A, which accounts for 55wt% of the total amount of raw coal, and 45wt% coal B are ground into pulverized coal of less than 200 mesh in a mill, and sent to a briquetting machine with a working pressure of 26MP to form briquettes. After primary crushing and secondary Screening after crushing;
[0043] Qualified pellets (3mm ~ 10mm) are subjected to oxidation treatment and carbonization treatment in sequence, and the oxidation treatment conditions are: oxidize the pellets for 3 hours at 230-250°C with air as the oxidant in an electrically heated external heating converter Treatment; the carbonization treatment conditions are as follows: carbonize the material for 2.5 hours at 500-550°C in an electric heating external heating converter, and control the oxygen concentration in the furnace atmosphere below 5vol%.
[0044] After cooling, the carbonized material obtained is soaked in 10% potassium nitrate solution for 2 hours, dried (the nitrate content is about 0.96%), an...
Embodiment 3
[0046] Coal A and 50wt% coal B, which account for 50wt% of the total amount of raw coal, are ground into pulverized coal of less than 200 mesh in a mill, and sent to a briquetting machine with a working pressure of 26MP to form briquettes. After primary crushing and secondary Screening after crushing;
[0047] Qualified pellets (3mm ~ 8mm) are subjected to oxidation treatment and carbonization treatment in sequence. The oxidation treatment conditions are: oxidize the pellets for 3 hours at 230-250°C with air as the oxidant in an electrically heated external heating converter Treatment; the carbonization treatment conditions are as follows: carbonize the material for 2.5 hours at 500-550°C in an electric heating external heating converter, and control the oxygen concentration in the furnace atmosphere below 5vol%.
[0048] After cooling, the obtained carbonized material is soaked in a solution of 15% calcium nitrate and magnesium nitrate at a mass concentration of 1:1 for 2 hou...