Silicon wafer for electronic components and method for manufacturing the same

By epitaxially growing a silicon layer on a carrier substrate and introducing p-type and n-type doping materials, the problems of non-uniform doping and high cost of silicon wafers in the prior art are solved, realizing low-cost and high-precision silicon wafer manufacturing, which is suitable for high-efficiency solar cells and large-area light-emitting devices.

CN109075027BActive Publication Date: 2024-10-25NEXWAFE GMBH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN201780024879.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-04-22
Filing Date
2017-04-11
Publication Date
2024-10-25
Estimated Expiration
2037-04-11

AI Technical Summary

Technical Problem

Existing technologies make it difficult to manufacture silicon wafers with low or no electrical activity net doping with high precision and low cost, and the inhomogeneity of doped materials and expensive process steps lead to high costs.

Method used

By epitaxially growing a silicon layer on a carrier substrate and introducing p-type and n-type doping materials, a doping concentration greater than 1×10¹³ cm⁻³ is formed. Combined with gas flow rate control and selection of doping materials, precise control of net electroactive doping is achieved.

Benefits of technology

It enables high-precision, low-cost manufacturing of silicon wafers, reduces the precision requirements of gas composition in the process chamber, simplifies the process, and is suitable for manufacturing high-efficiency solar cells and large-area light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109075027B_ABST
    Figure CN109075027B_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a silicon wafer for electronic components, the method comprising the steps of epitaxially growing a silicon layer on a carrier substrate and separating the silicon layer from the carrier substrate as a silicon wafer, wherein during the epitaxial growth, at least one p-type doping material and at least one n-type doping material are introduced into the silicon layer. The invention is characterized in that the introduction of the doping material into the silicon layer is carried out so as to form a silicon wafer having a thickness of each greater than 1×10 14 cm ‑3 electrically active p-type doped and electrically active n-type doped silicon layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a silicon wafer for manufacturing electronic components according to the preamble of claim 7 and a method for manufacturing the silicon wafer according to the preamble of claim 1. Background Art

[0002] For large-area electronic components, such as large-area light-emitting elements or photovoltaic solar cells, low-cost semiconductor wafers with high electronic performance are required, because in such components, the material costs of the semiconductor wafers account for a large proportion of the overall product costs. Summary of the invention

[0003] The object of the present invention is to improve the performance of a silicon wafer. This object is achieved by the use of the method according to claim 1, the silicon wafer according to claim 7, and the device for epitaxial growth of a silicon layer according to claim 15.

[0004] The silicon wafer according to the invention is preferably produced by means of the method according to the invention, in particular the preferred embodiments thereof. The method according to the invention is preferably used to produce the silicon wafer according to the invention, in particular the preferred embodiments thereof.

[0005] The invention is based on the recognition that the electrically active net doping of silicon wafers represents a decisive target value in the production of such wafers, which target value could not be preset with high precision to date or required expensive process steps. In particular, the production of silicon wafers with a low electrically active net doping or, in the extreme case, no electrically active net doping could not be carried out with high precision or the required process steps were costly.

[0006] In this case, the electrically active net doping describes the concentration of the dopant material that contributes to the conductivity of the semiconductor material, as opposed to the total doping (which describes the total amount of all dopant atoms introduced into the semiconductor layer). In this case, the net doping is always less than the total doping due to the compensation of dopant atoms of opposite polarity (n-type dopant and p-type dopant) that do not contribute to the conductivity.

[0007] Research and problem analysis of existing manufacturing methods have shown that during the production of silicon wafers, undesirable side effects of the p-type and n-type doping of the silicon wafers often occur. In particular, doping residues in the raw materials to be processed or in the process environment lead to the presence of difficult-to-prevent and influential doping components in the wafer. As a result, a lower precision in the preset electrically active target doping of the silicon wafers must be accepted - especially with a desired low electrically active net doping, or in extreme cases the goal is to produce silicon wafers without electrically active doping - or it must be done with the help of expensive processes to avoid the inclusion of doped materials in the production process, especially in the process chambers in which the silicon is processed into silicon wafers.

[0008] Therefore, according to the teachings known to date for producing silicon wafers, attempts have always been made to arrange the electrically active doping material only in the range in which an electrically active net doping is desired. This is particularly true for the known mold production processes, since the above-described disadvantages arise, in particular, due to the different precipitation coefficients of the individual doping materials. In particular, these disadvantages lead to undesirable changes in the net doping concentration.

[0009] In contrast, the silicon wafer according to the invention for producing electronic components has a p-type doping by means of at least one p-type doping material and an n-type doping by means of at least one n-type doping material.

[0010] It is obvious that the electroactive concentrations of p-type and n-type doping are greater than 1×10 13 cm -3 .

[0011] Therefore, in the silicon wafer according to the present invention, a relatively high proportion of the 13 cm -3 The use of these doping materials of opposite doping types results in a compensation of the electrically active doping, so that the electrically active net doping is approximately given by the difference in the electrically active density of the two oppositely doping materials.

[0012] Therefore, it is assumed that at least 1×10 13 cm -3 The base level of n-type doping is determined, and the electrically active net doping of the wafer is determined via the difference between the n-type doping concentration and the p-type doping concentration, and vice versa.

[0013] This brings significant advantages:

[0014] Since 1×10 13 cm -3 The impurities significantly below the basic level have no effect or only a negligible effect on the conductivity of the semiconductor layer. 13 cm -3 If the base level is smaller than that of the process chamber, significantly greater inaccuracies in the presence of doping materials can be tolerated in the process chamber during silicon wafer manufacturing. This leads to a significant reduction in the accuracy requirements for the gas composition in such process chambers and thus saves costs.

[0015] Furthermore, the invention enables cost-effective and high-precision production of silicon wafers with no or little electrically active net doping: it is significantly simpler in terms of process technology and can be produced at a rate of at least 1×10 14 cm -3The formation of a balanced electrically active p-type doping and an electrically active n-type doping or a difference between p-type and n-type doping in the doping level of 100 Å leads to a low electrically active net doping. This is caused on the one hand by the impurities already mentioned, which lead to electrically active doping.

[0016] Likewise, mixing of dopants in the process chamber can be handled more simply in terms of control technology, which results in a ratio of greater than 1×10 14 cm -3 The electrically active doping is therefore greater than the previously preset value. Therefore, in general, the material flow rate, in particular the gas flow rate when introducing the doping material into the process chamber of the present invention, is easier to handle, because relatively large concentrations of p-type doping material and n-type doping material are selected to reach at least 1×10 14 cm -3 basic level.

[0017] Furthermore, the object mentioned at the outset is achieved by a method for producing a silicon wafer for electronic components according to claim 1. The method according to the invention has the method steps of epitaxially growing a silicon layer on a carrier substrate and separating the silicon layer from the carrier substrate as a silicon wafer. During the epitaxial growth, at least one p-type doping material and at least one n-type doping material are introduced into the silicon layer to form an electrically active doping.

[0018] It is obvious that the introduction of doping materials into the silicon layer is achieved so as to form a silicon layer having a density greater than 1×10 13 cm -3 electrically active p-type doped and electrically active n-type doped silicon layers.

[0019] The silicon wafer produced in this way therefore has the advantages described above. In addition, the described method for epitaxially growing a silicon layer on a carrier substrate and separating the silicon layer from the carrier substrate as a silicon wafer is particularly suitable for producing such a silicon wafer.

[0020] To produce silicon wafers, the method widely used to date is to produce semiconductor wafers from silicon blocks (“casting molds”) by means of sawing methods. These casting molds are crystallized from molten semiconductor.

[0021] The crystallization is governed by diffusion processes which, according to Scheil's law, lead to an inhomogeneous distribution of the doping material in the crystal. The change in concentration is element-specific and can only be effected in a continuous crystallization process with considerable effort. Therefore, only with considerable technical effort can a stable net doping be achieved in the case of crystallization by increasing the basic doping level of the n-type doping as well as the p-type doping, but there is still a significantly increased inhomogeneity of the doping level over the length of the crystal.

[0022] The method of epitaxially growing a silicon layer on a carrier substrate and subsequently separating the silicon layer into silicon wafers is known per se and is described, for example, in the document “R. Brendel, Review of Layer Transfer Processes for Crystalline Thin-Film Silicon Solar Cells. Japanese Journal of Applied Physics, 2001, 40(7R), p. 4431”.

[0023] The method according to the invention therefore improves the known method for producing silicon wafers by means of epitaxial growth by providing during growth not only at least one p-type doping material but also at least one n-type doping material, so that at least 1×10 13 cm -3 The electrically active p-type doping and at least 1×10 13 cm -3 Electrically active n-type doping.

[0024] If, in a preferred embodiment, a higher basic level of electrically active p-type and n-type doping is selected, in particular so that the silicon wafer has a respective thickness of more than 5×10 14 cm -3 , preferably 1×10 15 cm -3 , especially 5×10 15 cm -3 The advantages mentioned above are enhanced if the p-type doping and n-type doping have an electrically active concentration of 1×10 14 cm -3 to 1×10 16 cm -3 It is also advantageous if the method according to the invention is used to produce silicon wafers having such parameters.

[0025] As already mentioned, it is possible to obtain a resolution of at least 1 × 10 14 cm -3 The base levels of p-type doping and n-type doping produce a low electrically active net doping.

[0026] Therefore, the silicon wafer according to the invention is preferably manufactured as a high-resistance wafer as mentioned above. In this advantageous embodiment, the silicon wafer has an electrically active net doping such that the silicon wafer has a specific resistance of greater than 1 Ωcm, preferably greater than 5 Ωcm, in particular greater than 20 Ωcm. Such a high-resistance wafer is particularly suitable for use as a high-efficiency solar cell, in which the electrical conductivity is determined by the charge carriers generated by light absorption under illumination and, secondarily, only by the doping atoms introduced into the material.

[0027] Alternatively or additionally, the silicon wafer preferably utilizes at least 5×10 14 cm -3 , especially in 5×10 14 cm -3 to 1×10 16 cm -3 In the range, preferably in the range of 5×10 14 cm -3 to 5×10 15 cm -3 The electrically active net doping describes the difference between the electrically active p-type doping and the electrically active n-type doping, wherein the doping type with the lower doping is respectively subtracted from the doping type with the higher doping to determine the electrically active net doping (the doping type with the higher doping).

[0028] Thus, in an advantageous embodiment, this manufacturing method enables the production of silicon wafers having the parameters mentioned previously.

[0029] When producing electronic components, a precisely defined doping, in particular a precisely defined electrically active net doping, is desirable since this can significantly influence the electronic properties, such as charge carrier mobility or charge carrier recombination rate.

[0030] Therefore, as described above, the electrically active p-type doping and n-type doping in the wafer according to the invention are at least 1×10 14 cm -3 The basic level of the silicon wafer also enables the course of the electrically active net doping to be precisely predefined, in particular in the thickness direction, i.e. perpendicularly to the front side of the silicon wafer. Advantageously, the silicon wafer thus has an electrically active net doping that is substantially constant in the thickness direction. The method is therefore advantageously designed such that the silicon layer forms an electrically active net doping that is substantially constant in the thickness direction.

[0031] However, optionally, the possibility of accurately presetting the electrically active net doping also opens up the possibility of purposefully presetting the course of the electrically active net doping in the thickness direction. Therefore, in an advantageous embodiment, the silicon wafer has an electrically active net doping like this, which has a step-like course of change or a linear course of change in the thickness direction. This is particularly advantageous for forming a so-called "back surface field" (BSF) or drift field in photovoltaic solar cells, which can effectively reduce charge carrier recombination at the wafer surface or in the bulk. The same applies to the so-called "front surface field" (FSF).

[0032] The method according to the invention is therefore preferably designed such that the silicon layer has such a profile of the electrically active net doping.

[0033] Thus, in particular, a profile of the electrically active net doping in the thickness direction can be achieved which differs from the typical profile when manufacturing silicon wafers from a mold. It is generally desirable to avoid such typical exponential profiles, in particular profiles according to Scheil's law. Thus, the silicon wafer according to the invention advantageously has an electrically active net doping with a non-exponential profile in the thickness direction, in particular an electrically active static doping which does not vary according to Scheil's law. The production of such a silicon wafer is achieved in particular by means of the method according to the invention.

[0034] In the method according to the invention, preferably a silicon layer with a thickness of at least 50 μm, in particular at least 100 μm, particularly preferably with a thickness in the range of 50 μm to 350 μm is used. Therefore, the silicon wafer according to the invention advantageously has a thickness of at least 50 μm, in particular at least 100 μm, particularly preferably with a thickness in the range of 50 μm to 350 μm.

[0035] It is particularly simple and therefore cost-effective in terms of process technology if, in a preferred embodiment, in the method according to the invention for epitaxially growing a silicon layer in a process chamber, a gas containing n-type dopant, p-type dopant and silicon is introduced simultaneously.

[0036] It is also particularly simple and cost-effective from a process technology perspective if, in a preferred embodiment, at least one doping material is introduced into the process via a fixed doping source, for example a phosphorus glass or boron glass or a ceramic containing phosphorus or boron.

[0037] The silicon wafer according to the present invention is particularly suitable for manufacturing large-area semiconductor components, such as large-area light-emitting components, such as LEDs.

[0038] The silicon wafer according to the invention is preferably used for the production of photovoltaic solar cells, since, in particular in the case of photovoltaic solar cells, the total costs depend significantly on the quality and cost of the semiconductor layers used, and, in particular in the case of photovoltaic solar cells, the electrically active net doping needs to be precisely preset. Therefore, the silicon wafer is preferably used for the production of photovoltaic solar cells, in particular the silicon wafer covers at least 10×10 cm 2 The front and back sides of the silicon wafer each have an area of ​​at least 10×10 cm 2 Alternatively or additionally, it is advantageous if the silicon wafer has a charge carrier lifetime of at least 300 μs, preferably at least 500 μs, and / or if the silicon wafer has a thickness in the range of 30 μm to 300 μm, in particular in the range of 50 μm to 200 μm.

[0039] As described above, a device for epitaxially growing a silicon layer on a carrier substrate is known. The object mentioned at the outset is therefore further achieved by using a device for epitaxially growing a silicon layer, wherein the device has a process chamber for accommodating the carrier substrate and a heating device for heating the process chamber and at least one gas inlet into the process chamber. The device is used to produce silicon wafers with p-type doping by means of at least one p-type doping material and silicon wafers with n-type doping by means of at least one n-type doping material, wherein the electrical activity density of the p-type doping and the n-type doping is each greater than 1×10 14 cm -3 . BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Other preferred features and embodiments are described below with reference to the accompanying drawings of exemplary embodiments.

[0041] Figure 1 An exemplary embodiment of an apparatus for carrying out an exemplary embodiment of the method according to the invention is shown. DETAILED DESCRIPTION

[0042] Figure 1 The device for epitaxial growth of silicon layers is shown. The device has a process chamber 3 for receiving a carrier substrate 1. The carrier substrate 1 can be moved into and out of the process chamber 3 by means of a conveyor device 6 designed as a conveyor belt. For this purpose, the process chamber 3 has a lock.

[0043] The process chamber 3 can be heated by means of the heating device 5. Furthermore, a gas flow can be introduced into the process chamber 3 via the gas inlet 4. Gas can be removed from the process chamber via the gas outlet.

[0044] Figure 1The device shown in and its operation can be implemented in a manner known per se, in particular as described in document WO 2012 / 084187 or document DE 10 2015 118 042.

[0045] In an exemplary embodiment of the method according to the invention, firstly a surface of the carrier substrate 1 (located at Figure 1 The carrier substrate is made porous. The porousization of the carrier substrate is known per se and is used in particular to be able to separate the epitaxially grown silicon layer from the carrier substrate. The carrier substrate itself is likewise made of silicon.

[0046] The carrier substrate pretreated in this way is introduced into the process chamber 3 by means of the transport device 6 until Figure 1 . Subsequently, epitaxial growth of the silicon layer 2 is achieved, wherein the process chamber 3 is heated by means of a heating device 5 and chlorosilane gas or silane gas containing silicon and, for example, diborane gas (which contains boron as a p-type dopant) and phosphine gas (which contains phosphorus as an n-type dopant) are introduced via a gas inlet 4. Optionally, a plurality of gas inlets may be provided, in particular one or more separate gas inlets may be provided for each gas.

[0047] The epitaxial growth of the silicon layer 2 is carried out using essentially known process parameters. The significant difference is that the gas containing the p-type dopant and the n-type dopant is supplied in such a high concentration that the silicon layer has a density of currently 1×10 14 cm -3 The electrically active p-type doping and current is 6×10 14 cm -3 Electrically active n-type doping.

[0048] Therefore, the silicon layer has a 5×10 14 cm -3 The n-doping type is electrically active net doping and thus forms a high-resistance silicon layer with approximately 10 Ωcm.

[0049] Typically, process parameters that may be used for this process are a process temperature of 1050°C, a hydrogen flow rate of 50 standard liters / minute, 1 standard liter / minute of chlorosilane, 0.002 standard liters / minute of phosphine dissolved in hydrogen, and 0.001 standard liters / minute of diborane dissolved in hydrogen.

[0050] Subsequently, the carrier substrate 1 with the silicon layer 2 is removed from the process chamber 3 by means of a transport device 6 and the silicon layer 2 is separated from the carrier substrate 1. The separated silicon layer 2 thus corresponds to an embodiment of a silicon wafer according to the invention.

[0051] The carrier substrate has an approximately square surface with a side length of 10 cm in the present case, so that the silicon wafer produced also has approximately this size. In the present case, the silicon wafer produced has a thickness of 100 μm.

[0052] In this exemplary embodiment, the concentrations of both the n-type doping material and the p-type doping material remain constant during epitaxial growth, so that the silicon layer 2 has a substantially uniform thickness in the thickness direction (perpendicular to the substrate). Figure 1 The front side of the top silicon layer 2 in the middle has a constant active net doping.

[0053] Optionally, in other embodiments, the gas flow can be changed during the epitaxial growth so that the silicon layer 2 has an electrically active net doping that has a step-like or linear variation in the thickness direction. The preferred variation is from 1×10 14 cm -3 The electrically active net doping changes stepwise or linearly to 1×10 15 cm -3 The electrically active net doping.

[0054] In the step-wise change, starting from a lower doping level, steps of 10-30% relative concentration change are advantageous.

[0055] The three aforementioned profiles, ie the constant, step-shaped or linear profile of the net active doping, have in common that there is no typical exponential profile during the mold production process, in particular no profile according to Scheil's law.

Claims

1. A method for producing a silicon wafer for electronic components, the method comprising the method steps of epitaxially growing a silicon layer (2) on a carrier substrate (1) and separating the silicon layer (2) from the carrier substrate (1) for use as a silicon wafer, wherein: During the epitaxial growth, at least one p-type doping material and at least one n-type doping material are introduced into the silicon layer (2), The invention is characterized in that the at least one p-type doping material and the at least one n-type doping material are introduced into the silicon layer (2) so as to form the silicon layer (2) having an electrically active p-type doping and an electrically active n-type doping, wherein the concentrations of the electrically active p-type doping and the electrically active n-type doping are each between 1×10 14 cm -3 Up to 1×10 16 cm -3 In the range of at least 1×10 14 cm -3 The electrically active net doping of the silicon wafer enables significantly greater inaccuracies in the presence of doping materials to be tolerated in the process chamber during silicon wafer manufacturing.

2. The method according to claim 1, characterized in that: The silicon layer (2) is formed with electrically active net doping, so that the silicon wafer has a sheet resistance greater than 1Ωcm.

3. The method according to claim 2, characterized in that The sheet resistance of the silicon wafer is greater than 5Ωcm.

4. The method according to claim 2, characterized in that: The thin film resistance of the silicon wafer is greater than 20Ωcm.

5. The method according to claim 1, characterized in that The electrically active net doping is located at 1×10 14 cm -3 to 1×10 16 cm -3 In range.

6. The method according to claim 1, characterized in that The electrically active net doping is within 5×10 14 cm -3 to 1×10 15 cm -3 In range.

7. The method according to any one of the preceding claims, characterized in that The silicon layer (2) is formed with a substantially constant electrically active net doping in the thickness direction.

8. The method according to any one of the preceding claims, characterized in that Formed with each larger than 5×10 14 cm -3 The electrically active concentrations of p-type doping and n-type doping in the silicon layer (2).

9. The method according to claim 8, characterized in that The electroactive concentration is 1×10 15 cm -3 .

10. The method according to claim 8, characterized in that The electroactive concentration is 5×10 15 cm -3 .

11. The method according to any one of the preceding claims, characterized in that The epitaxially applied silicon layer (2) has a thickness of at least 50 μm.

12. The method according to any one of the preceding claims, characterized in that The epitaxially applied silicon layer (2) has a thickness of at least 100 μm.

13. The method according to any one of the preceding claims, characterized in that In order to epitaxially grow the silicon layer (2) in the process chamber (3), a gas containing the n-type doping material, the p-type doping material and silicon is introduced simultaneously.

14. A silicon wafer for manufacturing electronic components and manufactured using the method according to any one of claims 1 to 13, the silicon wafer having an epitaxially grown silicon layer (2), at least one p-type doping material and at least one n-type doping material being introduced into the silicon layer (2) during the epitaxial growth, so that the silicon layer (2) is a silicon layer having electrically active p-type doping and electrically active n-type doping; The electrically active concentrations of the electrically active p-type doping and the electrically active n-type doping are each within a range of 1×10 14 cm -3 Up to 1×10 16 cm -3 In the range of at least 1×10 14 cm -3 The electrically active net doping of the silicon wafer enables significantly greater inaccuracies in the presence of doping materials to be tolerated in the process chamber during silicon wafer manufacturing.

15. The silicon wafer according to claim 14, characterized in that The silicon wafer has an electrically active net doping such that the silicon wafer has a sheet resistance greater than 1 Ωcm.

16. The silicon wafer according to claim 15, characterized in that The silicon wafer has a sheet resistance greater than 5Ωcm.

17. The silicon wafer according to claim 15, characterized in that The thin film resistance of the silicon wafer is greater than 20Ωcm.

18. The silicon wafer according to claim 14, characterized in that The electrically active net doping is within 5×10 14 cm -3 to 1×10 16 cm -3 In range.

19. The silicon wafer according to claim 14, characterized in that: The electrically active net doping is within 5×10 14 cm -3 to 5×10 15 cm -3 In range.

20. The silicon wafer according to any one of claims 14 to 19, characterized in that The silicon wafer has a substantially constant electrically active net doping in a thickness direction.

21. The silicon wafer according to any one of claims 14 to 19, characterized in that The silicon wafer has electrically active net doping, and the electrically active net doping has a step-like variation process or a linear variation process in a thickness direction.

22. The silicon wafer according to any one of claims 14 to 21, characterized in that The electrically active net doping has a non-exponential variation process in the thickness direction.

23. The silicon wafer according to any one of claims 14 to 21, characterized in that The electrically active net doping has a profile in the thickness direction that does not follow Scheil's law.

24. The silicon wafer according to any one of claims 14 to 23, characterized in that The electrical activity density of the electrically active p-type doping and the electrically active n-type doping is greater than 5×10 14 cm -3 .

25. The silicon wafer according to claim 24, characterized in that The electrical activity density of the electrically active p-type doping and the electrically active n-type doping is greater than 1×10 15 cm -3 .

26. The silicon wafer according to claim 24, characterized in that The electrical activity density of the electrically active p-type doping and the electrically active n-type doping is greater than 5×10 15 cm -3 .

27. The silicon wafer according to any one of claims 14 to 26, characterized in that The silicon wafer is designed to be used for manufacturing photovoltaic solar cells, and the silicon wafer covers at least 10×10 cm 2 and / or the silicon wafer has a charge carrier lifetime of at least 300 μs and / or the silicon wafer has a thickness in the range of 30 μm to 300 μm.

28. The silicon wafer according to claim 27, characterized in that The silicon wafer has a charge carrier lifetime of at least 500 μs.

29. The silicon wafer according to claim 27, characterized in that The silicon wafer has a thickness in the range of 50 μm to 200 μm.

30. A device for epitaxially growing a silicon layer (2), the device comprising a process chamber (3) for accommodating a carrier substrate, a heating device (5) for heating the process chamber (3) and at least one gas inlet (4) to the process chamber (3), the device being used for manufacturing a silicon wafer using a method according to any one of claims 1 to 13, the silicon wafer having the epitaxially grown silicon layer (2), the silicon layer (2) having at least one p-type doping material and at least one n-type doping material introduced during the epitaxial growth, so that the silicon layer (2) is a silicon layer having an electrically active p-type doping and an electrically active n-type doping, the electrically active concentrations of the electrically active p-type doping and the electrically active n-type doping being each in the range of 1×10 14 cm -3 Up to 1×10 16 cm -3 In the range of at least 1×10 14 cm -3 The electrically active net doping of the silicon wafer enables significantly greater inaccuracies in the presence of doping materials to be tolerated in the process chamber during silicon wafer manufacturing.

31. Use of a silicon wafer in manufacturing a photovoltaic solar cell, the silicon wafer comprising an epitaxially grown silicon layer (2), the silicon layer (2) comprising p-type doping by means of at least one p-type doping material and n-type doping by means of at least one n-type doping material, so that the silicon layer (2) is a silicon layer having electrically active p-type doping and electrically active n-type doping, wherein the electrically active concentrations of the p-type doping and the n-type doping are respectively within a range of 1×10 14 cm -3 Up to 1×10 16 cm -3 In the range of at least 1×10 14 cm -3 The electrically active net doping of the silicon wafer enables significantly greater inaccuracies in the presence of doping materials to be tolerated in the process chamber during silicon wafer manufacturing.

Citation Information

Patent Citations

  • Retaining device for substrates and method for coating a substrate

    WO2012084187A1

  • Method of forming power semiconductor devices with controllable integrated buffer

    CA2213840A1

  • Semiconductor crystal manufacture method

    CN101388336A

  • Silicon wafer and production method thereof

    CN102376749A

  • Fabrication process of semiconductor substrate

    CN1169025A