Well-formed casting mold
Through the combination of the casting mold made of self-hardened sand of furan resin and the accelerated cooling and vibration motor of cold iron, the problems of incomplete cast iron impeller molding and long stress removal time are solved, and the effects of high pass rate, low cost and rapid manufacturing are achieved.
Patent Information
- Application Number
- CN201910298043.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-04-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-04-15
AI Technical Summary
During the casting process of existing cast iron impellers, due to the long and thin blades, it is difficult to emptiate air when pouring iron, resulting in incomplete molding and low pass rate. Thickening of the blades requires increasing weight and cost, and the stress removal time is long.
The casting mold made of self-hardened sand of furan resin is connected to the upper and lower molds through studs, and a cold iron accelerated cooling and vibration motor is installed to ensure that the molten iron fills the cavity, reduces air retention, and eliminates stress through pressure and vibration.
It improves casting pass rate, reduces material and processing costs, shortens manufacturing time, and improves energy conversion efficiency.
Smart Images

Figure CN109822050B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of casting molds for cast iron impellers, and in particular relates to a casting mold with good molding. Background Art
[0002] Large cast iron impellers (abbreviated as impellers), such as turbine impellers, include a turntable and multiple blades. The blades are circumferentially distributed on the turntable. The blade size accuracy requirements are relatively high. A sleeve that matches the main shaft is provided in the middle of the turntable, and the gate position of the casting mold corresponds to the turntable. During pouring, the molten iron first fills the turntable, then the sleeve, and finally the blades. During the casting process, since the blades are long and thin, it is difficult to evacuate the air in the cavity corresponding to the blades when the molten iron is poured. The molten iron is not filled completely, the blades are not completely formed, and the impeller casting pass rate is low. After the pouring is completed, the molten iron at the blades solidifies first, and the specific part of the blade that solidifies first is uncontrollable. Usually, it starts to solidify from the far end of the blade, and then gradually solidifies toward the root of the blade connected to the turntable. This is the most ideal state. However, the volume of the blade shrinks during the solidification process, and the outer dimensions of the blade will shrink. Therefore, it is necessary to expand the size of the cavity where the blade is located so that the size of the blade obtained by casting exceeds the actual required size of the blade, and then the blade edge is precisely ground to obtain the actual size of the blade. The required size and complicated blade molding increase the processing cost of the impeller. Occasionally, the root of the blade connected to the turntable or the middle of the blade solidifies first. The iron block formed by solidification separates the far end of the blade from the flow channel. After the blade condenses and shrinks, the molten iron cannot be replenished to the far end of the blade in time, resulting in a gap on the edge of the far end of the blade. The far end of the blade will also become loose, and the casting is unqualified. To avoid this situation, it is usually necessary to thicken the blade, gradually thickening from the far end of the blade to the root of the blade. The thickness of the blade seriously exceeds the actual thickness required by the blade, which directly increases the weight of the impeller, not only increasing the material cost, but also increasing the power required to drive the impeller, and reducing the energy conversion efficiency of the impeller. After the impeller is cast, there is a large stress that needs to be eliminated. Due to the large size of the impeller, it is not suitable to be placed in the furnace for tempering to eliminate stress, so it usually relies on natural aging to eliminate stress, which takes at least 6 months, and the manufacturing speed of the impeller is slow. Therefore, the impellers cast by the existing casting molds have defects of low casting qualification rate, high processing cost and long manufacturing time, or have defects of low casting qualification rate, high material cost, low energy conversion efficiency and slow manufacturing speed. Summary of the invention
[0003] The object of the present invention is to provide a casting mold with good molding, which has the advantages of high casting qualification rate, low processing cost, low material cost, high energy conversion efficiency and fast manufacturing speed.
[0004] The technical solution of the present invention is as follows: a well-formed casting mold comprises an upper mold and a lower mold both made of furan resin self-hardening sand, the upper mold is connected to the lower mold by studs, the upper surface of the lower mold is provided with a cavity matching the shape of the impeller, a plurality of chills are inlaid in the cavity, the position of the chills corresponds to the distal end of the blade, a main flow channel is provided in the upper mold, the upper end of the main flow channel is located on the upper surface of the upper mold, the lower end of the main flow channel extends into the lower mold, the lower end of the main flow channel is connected to a plurality of circumferentially distributed branch channels, a gate is provided at the end of the branch channel, and the position of the gate corresponds to the inner wall of the sleeve.
[0005] In the aforementioned well-formed casting mold, the mold cavity includes a step hole that matches the shape of the turntable, the depth of the step hole is greater than the thickness of the turntable, a lower pressure plate is embedded in the bottom of the upper mold, and the lower part of the lower pressure plate is embedded in the step hole. An upper pressure plate is provided above the upper mold, and the upper pressure plate is connected to the lower pressure plate through multiple guide pillars. The upper mold is provided with guide holes that cooperate with the guide pillars.
[0006] In the aforementioned well-formed casting mold, a vibration motor is fixed on the upper pressing plate.
[0007] In the aforementioned well-formed casting mold, the stud passes through the upper mold and is connected to the lower mold, and the lower end of the stud is provided with a nut embedded in the lower mold.
[0008] In the aforementioned well-formed casting mold, there are four branch channels, which are distributed in a cross shape.
[0009] In the aforementioned well-formed casting mold, a skeleton surrounding the mold cavity is provided in the lower mold, and the distance between the mold cavity and the skeleton is 1-3 cm.
[0010] Compared with the prior art, the present invention adopts furan resin self-hardening sand to make the upper mold and the lower mold, so that the upper mold and the lower mold have good air permeability and rigidity. When molten iron is poured into the cavity, the air in the cavity corresponding to the blade can be discharged through the lower mold, and the molten iron can better fill the cavity position corresponding to the blade. The blade is well-formed and complete, and the casting qualification rate of the impeller is high.
[0011] By setting a cold iron to accelerate the cooling rate of the far end of the blade, it is ensured that the far end of the blade rises and solidifies first, and the far end of the blade and the flow channel are always kept unobstructed. The cavity vacancy caused by the solidification of the far end of the blade can be supplemented by the molten iron in the flow channel, ensuring that the cavity position corresponding to the far end of the blade can always be filled with molten iron. The blade is completely formed and there is no need to thicken the blade, which reduces the weight of the impeller, that is, reduces the material cost, and also reduces the power required to drive the impeller, thereby improving the energy conversion efficiency of the impeller.
[0012] When the molten iron pouring is completed and begins to solidify gradually, pressure is applied to the lower platen through the upper platen, and the casting is compacted under pressure to avoid looseness inside the casting. At the same time, the cavity position corresponding to the blade is always completely filled under pressure, and no cavity will be generated due to blade cooling. The size of the blade after forming is precise, and only the size of the cavity position corresponding to the blade needs to be the actual required size of the blade. The formed blade does not need to be precision ground, which reduces the processing cost of the impeller.
[0013] After the molten iron has completely cooled in the cavity, the vibrating motor is used to vibrate the casting. This first separates the casting from the cavity wall, making it easier to remove the casting from the mold. Second, the vibration motor eliminates some of the casting stress, reducing the subsequent natural aging time of the casting to about four months, thereby reducing the impeller manufacturing time.
[0014] Therefore, the present invention has the advantages of high casting qualification rate, low processing cost, low material cost, high energy conversion efficiency and fast manufacturing speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a front view of the present invention.
[0016] Figure 2 It is a top view of the runner.
[0017] Figure 3 It is a schematic diagram of the skeleton structure.
[0018] Figure 4 This is the front view of the impeller.
[0019] Figure 5 This is a top view of the impeller.
[0020] The markings in the attached drawings are: 1-upper mold, 2-lower mold, 3-vibration motor, 11-stud, 13-main channel, 14-dividing channel, 15-gate, 16-lower pressure plate, 17-upper pressure plate, 18-guide column, 19-nut, 21-cold iron, 22-skeleton, 31-blade, 32-sleeve, 33-turntable. DETAILED DESCRIPTION
[0021] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0022] Example. A well-formed casting mold, such as Figure 1As shown, it includes an upper mold 1 and a lower mold 2 both made of furan resin self-hardening sand. The upper mold 1 and the lower mold 2 are both glued together with furan resin self-hardening sand. The upper mold 1 is connected to the lower mold 2 through a stud 11. The upper surface of the lower mold 2 is provided with a cavity matching the shape of the impeller. A plurality of chills 21 are embedded in the cavity. The position of the chills 21 corresponds to the distal end of the blade 31. A main flow channel 13 is provided in the upper mold 1. The upper end of the main flow channel 13 is located on the upper surface of the upper mold 1. The lower end of the main flow channel 13 extends into the lower mold 2. The lower end of the main flow channel 13 is connected to a plurality of circumferentially distributed branch channels 14. The end of the branch channel 14 is provided with a gate 15. The position of the gate 15 corresponds to the inner wall of the sleeve 32.
[0023] The cavity includes a stepped hole that matches the shape of the turntable 33, and the depth of the stepped hole is greater than the thickness of the turntable 33. A lower pressure plate 16 is embedded in the bottom of the upper mold 1, and the lower part of the lower pressure plate 16 is embedded in the stepped hole. An upper pressure plate 17 is provided above the upper mold 1, and the upper pressure plate 17 is connected to the lower pressure plate 16 through a plurality of guide pillars 18. The upper mold 1 is provided with guide holes that cooperate with the guide pillars 18.
[0024] A vibration motor 3 is fixed on the upper pressing plate 17 , and the exciting force of the vibration motor 3 is 180 kN.
[0025] The stud 11 passes through the upper die 1 and is connected to the lower die 2 . The lower end of the stud 11 is provided with a nut 19 embedded in the lower die 2 .
[0026] There are four branch channels 14, which are distributed in a cross shape.
[0027] The lower mold 2 is provided with a skeleton 22 surrounding the mold cavity, the distance between the mold cavity and the skeleton 22 is 1-3 cm, the skeleton 22 is made of carbon steel perforated plate, is cylindrical, and has a wall thickness of more than 4 mm. The skeleton 22 is used to enhance the strength of the lower mold 2 to prevent the lower mold 2 from breaking under pressure.
[0028] Casting steps: a. By weight, 100 parts of QT450-10 cast iron are melted in a 2T medium frequency induction furnace, 1.2 parts of graphite and 0.6 parts of inoculant are added, and stirred evenly to obtain molten iron at a temperature of 1380°C.
[0029] b. The molten iron reaches the cavity through the main channel 13, the branch channel 14, and the gate 15 in sequence. After cooling for 1-1.5 hours or more than half of the molten iron in the cavity solidifies, a certain pressure is applied to the upper plate 17 by a press until the molten iron is completely cooled. The pressure varies according to the size and shape of the impeller. The larger the impeller, the greater the pressure applied. The specific pressure value is based on the size of the obtained blade 31 and the cavity size corresponding to the blade 31. The deviation is no more than 0.1% (the deviation is no more than 0.1%, which means that the cavity position size corresponding to the blade is the blade size). The pressure value can be obtained through several tests.
[0030] c. Start the vibration motor 3 and stop after working for 3-5 hours.
[0031] d. Loosen the stud 11, take out the casting, and get the finished product after cleaning.
[0032] Therefore, the present invention has the advantages of high casting qualification rate, low processing cost, low material cost, high energy conversion efficiency and fast manufacturing speed.
Claims
1. A well-formed casting mold, characterized by: The invention comprises an upper mold (1) and a lower mold (2) both made of furan resin self-hardening sand, wherein the upper mold (1) is connected to the lower mold (2) via a stud (11), the upper surface of the lower mold (2) is provided with a cavity matching the shape of the impeller, a plurality of cold irons (21) are embedded in the cavity, and the position of the cold irons (21) corresponds to the distal end of the blade (31), a main flow channel (13) is provided in the upper mold (1), the upper end of the main flow channel (13) is located on the upper surface of the upper mold (1), the lower end of the main flow channel (13) extends into the lower mold (2), the lower end of the main flow channel (13) is connected to a plurality of circumferentially distributed branch flow channels (14), the end of the branch flow channel (14) is provided with a gate (15), and the position of the gate (15) corresponds to the inner wall of the shaft sleeve (32); The mold cavity comprises a stepped hole matching the shape of the turntable (33), the depth of the stepped hole being greater than the thickness of the turntable (33), a lower pressing plate (16) being embedded in the bottom of the upper mold (1), the lower part of the lower pressing plate (16) being embedded in the stepped hole, an upper pressing plate (17) being provided above the upper mold (1), the upper pressing plate (17) being connected to the lower pressing plate (16) via a plurality of guide pillars (18), and a guide hole matching the guide pillars (18) being provided on the upper mold (1); A vibration motor (3) is fixed on the upper pressing plate (17). When the molten iron is completely cooled in the mold cavity to form a casting, the vibration motor (3) applies a certain vibration to the casting, so as to facilitate the removal of the casting from the mold and reduce the subsequent natural aging time of the casting; The lower mold (2) is provided with a frame (22) surrounding the mold cavity, and the distance between the mold cavity and the frame (22) is 1-3 cm.
2. The well-formed casting mold according to claim 1, characterized in that: The stud (11) passes through the upper die (1) and is connected to the lower die (2). The lower end of the stud (11) is provided with a nut (19) pre-buried in the lower die (2).
3. The well-formed casting mold according to claim 1, characterized in that: The number of the branch flow channels (14) is four, which are distributed in a cross shape.