Connecting structure and method for manufacturing connecting structure
By placing conductive particles and insulating resin composition on the electrode, and forming conductive paths and insulating layers by pressing and photocuring, the anisotropic conductive film has been solved by poor conduction and short circuit in high-fine and high-density connections. Problem, high precision and reliable electrode connection are achieved.
Patent Information
- Application Number
- CN201910082217.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-01-31
- Filing Date
- 2019-01-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-01-28
AI Technical Summary
When the existing anisotropic conductive film is connected to a circuit in a highly refined and dense electronic device, irregular arrangement of conductive particles leads to poor conduction and short circuit problems, and the difference in thermal expansion coefficient caused by the heating and curing connection method leads to electrodes. Offsets are difficult to eliminate.
通过在电极上配置导电性粒子和绝缘性树脂组合物,并通过按压和光固化使其固化,形成导电路径和绝缘层,确保对向电极的导电性和邻接电极的绝缘性,避免加热固化连接法 thermal expansion problem.
Reliable conductive connection between high-fine and high-density electrodes is realized, short circuit is suppressed, and electrodes with different thermal expansion coefficients are connected with high precision, improving the reliability and accuracy of the connection.
Smart Images

Figure CN110197819B_ABST
Abstract
Description
Technical Field
[0001] One embodiment of the present invention relates to a connection structure having an electrode connection structure formed of a conductive composition, and a method for producing the connection structure. Background Art
[0002] When electronic components such as integrated circuits are mounted on substrates, such as COG (Chip on Glass) connections that directly connect integrated circuits to glass substrates of liquid crystal displays, and FOG (Film on Glass) connections that connect flexible printed substrates to glass substrates of flat panel displays, anisotropic conductive films (ACF) containing conductive particles are generally widely used. Anisotropic conductive films are films of thermosetting resins in which fine conductive particles are dispersed. By sandwiching the anisotropic conductive film between aligned electrodes and performing thermocompression bonding, the conductive particles located between the electrodes can form a conductive path. On the other hand, the insulating properties of thermosetting resins can be used to suppress short circuits of adjacent electrodes in the surface direction of the substrate. That is, the anisotropic conductive film has the anisotropy of "forming conductivity in the pressurized direction (direction of the two electrodes) and maintaining insulation in the non-pressurized direction (surface direction of the substrate)". Due to such characteristics, the anisotropic conductive film can connect a plurality of electrodes provided on an integrated circuit, a printed substrate, a glass substrate, etc. in batches, and can maintain the insulation of electrodes adjacent to each other in the surface direction of the substrate.
[0003] However, with the high precision and high density of the connection circuits in electronic devices in recent years, the reliability of the connection using anisotropic conductive films has become a problem. That is, if the size of the electrode to be connected becomes smaller, the number of conductive particles that contribute to conduction between a pair of electrodes will decrease, and the connection reliability between the electrodes cannot be fully obtained. In addition, if the distance between adjacent electrodes in the surface direction of the substrate becomes narrower, the conductive particles and the adjacent electrodes will contact each other, and the insulation reliability cannot be fully obtained. For this reason, Patent Document 1 discloses an anisotropic conductive film in which the conductive particles are dispersed by applying a magnetic field or the like, thereby being separated from other conductive particles.
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-167106 Summary of the invention
[0007] [Problems to be solved by the invention]
[0008] However, in anisotropic conductive films, when the substrates are thermally pressed together, the arrangement of the conductive particles is irregular and scattered, so that it is not possible to fully eliminate the poor conduction caused by the absence of conductive particles between electrodes and the short circuit caused by the conductive particles contacting between adjacent electrodes. Furthermore, since a heat curing connection method is adopted, in principle, a dimensional change caused by the difference in thermal expansion coefficients between the upper and lower substrates occurs, and it is not possible to eliminate the problem of the electrodes formed on the upper and lower substrates being offset from each other.
[0009] One embodiment of the present invention is completed in view of the existing problems as described above, and one of its purposes is to ensure the conductivity between opposing electrodes through a simple process and to prevent adjacent electrodes from short-circuiting even if the electrodes arranged on an integrated circuit, a printed substrate, a glass substrate, etc. are highly refined and highly dense.
[0010] [Methods for solving the problem]
[0011] A method for preparing a connecting structure according to one embodiment of the present invention comprises the following steps: disposing a first composition on a first surface of a first component provided with a first electrode, and disposing conductive particles on the first electrode; disposing a second composition overlapping with the first composition in an area other than the first electrode of the first surface; disposing the first surface and the second surface of a second component provided with the second electrode facing each other in a manner such that "the first composition and the conductive particles contact the second electrode, and the second composition contacts the area other than the second electrode of the second surface"; pressing the first component and the second component; and curing the first composition and the second composition.
[0012] A method for preparing a connecting structure according to one embodiment of the present invention includes the following steps: configuring a first composition on a first surface of a first component provided with a first electrode, and configuring conductive particles on the first electrode; configuring a second composition in an area other than the second electrode configured on a second surface of a second component; configuring the first surface and the second surface opposite to each other in a manner such that "the first composition and the conductive particles contact the second electrode, and the second composition overlaps the first composition in an area other than the first electrode of the first surface"; pressing the first component and the second component; and curing the first composition and the second composition.
[0013] A method for preparing a connecting structure according to one embodiment of the present invention comprises the following steps: configuring a second composition in an area other than a first electrode configured on a first surface of a first component; configuring the first composition on the first surface so as to overlap with the second composition, and configuring conductive particles on the first electrode; configuring the first surface and the second surface of the second component configured with the second electrode to face each other in a manner such that "the conductive particles contact the second electrode, and the first composition contacts the second surface"; pressing the first component and the second component; and curing the first composition and the second composition.
[0014] A method for preparing a connecting structure according to one embodiment of the present invention includes the following steps: configuring a second composition in an area other than a first electrode configured on a first surface of a first component; configuring the first composition on a second surface of a second component configured with a second electrode, and configuring conductive particles on the second electrode; configuring the first surface and the second surface to face each other in a manner such that "the first composition and the conductive particles contact the first electrode, and the second composition overlaps the first composition in an area other than the second electrode on the second surface"; pressing the first component and the second component; and curing the first composition and the second composition.
[0015] A connection structure according to one embodiment of the present invention includes: a first surface of a first component; a first electrode arranged on the first surface; a second surface of a second component facing the first surface; a second electrode arranged on the second surface opposite to the first electrode; a first resin and conductive particles arranged between the first electrode and the second electrode; and a first resin and a second resin arranged between an area other than the first electrode on the first surface and an area other than the second electrode on the second surface, wherein the first resin contacts the first surface, the second resin contacts the second surface, and the first resin is different from the second resin.
[0016] Effects of the Invention
[0017] According to one embodiment of the present invention, even if the electrodes arranged on the electronic components are highly refined and highly dense, the conductivity between the electrodes facing each other can be ensured by a simple process, and the short circuit between adjacent electrodes can be suppressed. Furthermore, since the heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a figure which shows the structure of the connection structure body which concerns on one Embodiment of this invention.
[0019] Figure 2It is a figure explaining the manufacturing method of the connection structure which concerns on one Embodiment of this invention.
[0020] Figure 3 It is a figure explaining the manufacturing method of the connection structure which concerns on one Embodiment of this invention.
[0021] Figure 4 It is a figure explaining the manufacturing method of the connection structure which concerns on one Embodiment of this invention.
[0022] Figure 5 It is a figure explaining the manufacturing method of the connection structure which concerns on one Embodiment of this invention.
[0023] Figure 6 It is a figure explaining the manufacturing method of the connection structure which concerns on one Embodiment of this invention.
[0024] Figure 7 It is a figure which shows the structure of the connection structure body which concerns on one Embodiment of this invention.
[0025] Figure 8 It is a figure explaining the manufacturing method of the connection structure which concerns on one Embodiment of this invention.
[0026] Fig. 9 It is a figure explaining the manufacturing method of the connection structure which concerns on one Embodiment of this invention.
[0027] Fig.10 It is a diagram showing the structure of a connection structure according to one embodiment of the present invention.
[0028] Fig.11 It is a diagram showing the structure of a connection structure according to one embodiment of the present invention.
[0029] Fig.12 It is a diagram showing the composition of a connection structure according to one embodiment of the present invention.
[0030] Fig.13 It is a diagram showing the structure of a connection structure according to one embodiment of the present invention. DETAILED DESCRIPTION
[0031] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings and the like. However, the present invention includes a variety of different forms and is not to be construed as limited to the embodiments illustrated below. In order to make the description clearer, the drawings attached to this specification sometimes schematically represent the width, thickness, shape, etc. of each part compared to the actual form, but this is only an example and does not necessarily limit the content of the present invention. In addition, in the present invention, when a specific element recorded in a certain drawing is the same as or corresponds to a specific element recorded in other drawings, the same symbol is sometimes marked (or a symbol obtained by marking a, b, etc. after the number recorded as the symbol), and repeated descriptions are appropriately omitted. Furthermore, the words "1st" and "2nd" marked on each element are convenient identifiers used to distinguish the elements, and have no further meaning unless otherwise specified.
[0032] In this specification, when a certain component or region is located "above (or below)" another component or region, unless otherwise specified, it includes not only the case where it is located directly above (or directly below) another component or region, but also the case where it is located above (or below) another component or region. That is, it also includes the case where another component is included between the above (or below) another component or region and the certain component or region.
[0033] In this specification, a connection structure in a COG connection in which an integrated circuit (second electronic component) is connected to a glass substrate of a liquid crystal display (first electronic component) is shown as an example. However, the present invention is not limited thereto, and a connection structure in a FOG connection in which a flexible printed substrate is connected to a glass substrate of a flat panel display may also be used. In this case, the second electronic component may also be a flexible printed substrate such as TAB (Tape Automated Bonding) or COF (Chip on Film).
[0034] <First embodiment>
[0035] [Structure of the connection structure]
[0036] Figure 1 The structure of a connection structure according to one embodiment of the present invention is shown. Figure 1 (A) is a plan view of a connection structure according to one embodiment of the present invention. Figure 1 (B) Yes Figure 1 (A) AA' cross-sectional view. Figure 1 (C) Yes Figure 1 (B) is an enlarged cross-sectional view of the conductive particles in the region B.
[0037] like Figure 1As shown in (A) and (B), the first electronic component 101 includes a terminal 104, a first insulating film 106, a second insulating film 108, and a first electrode 110 on the connection surface (first surface) of the first member 102. The second electronic component 111 is mounted on the connection surface (first surface) of the first electronic component 101. The second electronic component 111 includes a second electrode 114 on the connection surface (second surface) of the second member 112. The first surface of the first electronic component 101 and the second surface of the second electronic component 111 are arranged opposite to each other. The connection structure 100 is responsible for the physical connection between the first electronic component 101 and the second electronic component 111, and the electrical connection between the first electrode 110 and the second electrode 114. The connection structure 100 includes the first surface of the first member 102, the first electrode 110, the second surface of the second member 112, the second electrode 114, the conductive particles 10, the first resin 20, and the second resin 30.
[0038] A plurality of first electrodes 110 are arranged on the first surface of the first member 102. A second insulating film 108 is arranged in a region other than the region where the first electrodes 110 are arranged on the first surface of the first member 102. A plurality of second electrodes 114 corresponding to the plurality of first electrodes 110 are arranged on the second surface of the second member 112. An insulating film may also be arranged in a region other than the region where the second electrodes 114 are arranged on the second surface of the second member 112.
[0039] A plurality of first electrodes 110 and a plurality of second electrodes 114 are arranged opposite to each other. A plurality of conductive particles 10 and a first resin 20 are arranged between the first and second electrodes 110, 114. A plurality of conductive particles 10 are arranged in a plane direction (D2-D3 plane direction) between the first and second electrodes 110, 114. One conductive particle 10 is arranged in a direction (D1 direction) facing the first and second electrodes 110, 114 between the first and second electrodes 110, 114. Each conductive particle 10 contacts the first and second electrodes 110, 114. Figure 1As shown in (C), the conductive particle 10 is deformed by pressure in the direction of the electrodes facing each other (D1 direction) between the first electrode 110 and the second electrode 114 by the following method for producing a connection structure. That is, the distance between the first electrode 110 and the second electrode 114 in the direction of the electrodes facing each other (D1 direction) is approximately the same as the height of the conductive particle 10 in the direction of the electrodes facing each other (D1 direction). The height of the conductive particle 10 in the direction of the electrodes facing each other (D1 direction) is deformed by pressure by about 10% to 40%. By applying stress between the first electrode 110, the conductive particle 10, and the second electrode 114, the first resin 20 is excluded from the contact portion between the first electrode 110 and the conductive particle 10, and the contact portion between the second electrode 114 and the conductive particle 10. Furthermore, even if a natural oxide film is formed on the first electrode 110, the conductive particles 10, or the second electrode 114 and the surface is insulated, the first electrode 110 and the second electrode 114 can be pressed and bonded with each other with the conductive particles 10 interposed therebetween, thereby breaking through the natural oxide film and forming a conductive path. Furthermore, by deforming the conductive particles 10, the contact area between the first electrode 110 and the conductive particles 10 and the contact area between the second electrode 114 and the conductive particles 10 can be increased. By configuring in this way, the conductive particles 10 can electrically connect the first electrode 110 and the second electrode 114.
[0040] A plurality of conductive particles 10 are dispersed in the first resin 20 between the first electrode 110 and the second electrode 114. Each conductive particle 10 is surrounded by the first resin 20 in the surface direction (D2-D3 surface direction) between the first electrode 110 and the second electrode. The first resin 20 is an insulating resin. Therefore, the connection structure 100 has insulating properties in the surface direction (D2-D3 surface direction). However, a plurality of conductive particles 10 arranged between the first electrode 110 and the second electrode 114 facing each other and adjacent in the surface direction (D2-D3 surface direction) may also contact each other. When the conductive particles 10 adjacent in the surface direction (D2-D3 surface direction) contact each other, the adjacent conductive particles 10 are also electrically connected to each other. By configuring in this way, the conductive particles 10 can further reliably electrically connect the first electrode 110 and the second electrode 114 facing each other. The distance between adjacent conductive particles 10 can be appropriately controlled by the concentration of the conductive particles 10 mixed in the first composition 20 ′ described below.
[0041] like Figure 1As shown in (A) and (B), a plurality of conductive particles 10 and a first resin 20 are arranged between the first electrode 110 and the second electrode 114. In the present embodiment, when viewed from the opposite direction of the electrodes (the D1 direction), a plurality of conductive particles 10 and the first resin 20 are arranged on substantially the entire surface of the upper surface of the first electrode 110 (or the lower surface of the second electrode 114). The diameter of the conductive particles 10 observed in the opposite direction of the electrodes (the D1 direction) is within a range of 2 μm or more and 10 μm or less. The number of conductive particles 10 preferably arranged between the opposite first electrode 110 and the second electrode 114 is 7 / 400 μm. 2 20 or more / 400μm 2 When the number of the conductive particles 10 is less than several 7 / 400 μm 2 When the number of the conductive particles 10 is more than 20 / 400 μm, the connection resistance value may tend to vary. 2 In the case of , the pressure deformation of the conductive particles 10 may be reduced due to load dispersion, and the natural oxide film in the connection area may not be broken, resulting in increased connection resistance. 2 In the case of , the time-dependent change of the amount of compression deformation is likely to occur, and thus the time-dependent change of the connection resistance is likely to occur. By configuring in this way, the conductive particles 10 can reliably connect the first electrode 110 and the second electrode 114 facing each other, and can prevent short circuits between a plurality of first electrodes 110 adjacent in the plane direction (D2-D3 plane direction), between a plurality of second electrodes 114 adjacent in the plane direction (D2-D3 plane direction), and between the first electrode 110 and the second electrode 114 not facing each other.
[0042] In the present embodiment, the shape of the region where the conductive particles 10 and the first resin 20 are arranged observed in the opposite direction of the electrodes (D1 direction) is consistent with the first electrode 110 (or the second electrode 114) and is rectangular. However, this is not limited to this, and the shape of the region where the conductive particles 10 and the first resin 20 are arranged can be any shape as long as the above conditions are met.
[0043] The area of the region where the conductive particles 10 and the first resin 20 are arranged on the upper surface of one first electrode 110 (or the lower surface of the second electrode 114) may satisfy the above conditions, and may be appropriately adjusted by the area of the first electrode 110 (or the second electrode 114) and the size of the conductive particles 10. In addition, the number of conductive particles 10 arranged in the region where the conductive particles 10 and the first resin 20 are arranged may satisfy the above conditions, and may be appropriately adjusted by the size of the conductive particles 10 and the concentration of the conductive particles 10 mixed in the first composition 20' described below.
[0044] In the present embodiment, when viewed in the opposing direction of the electrodes (D1 direction), the first resin 20 is also arranged in the region other than the first electrode 110 of the first surface. When viewed in the opposing direction of the electrodes (D1 direction), the first resin 20 is also arranged between and around the plurality of first electrodes 110 of the first surface. On the other hand, when viewed in the opposing direction of the electrodes (D1 direction), the first resin 20 is not arranged at the end of the first surface. At this time, when viewed in the opposing direction of the electrodes (D1 direction), the conductive particles 10 are not arranged in the region other than the first electrode 110 of the first surface (the second electrode 114 of the second surface). That is, the conductive particles 10 are arranged on the first electrode 110 (or the second electrode 114).
[0045] The second resin 30 is further arranged between the first surface of the first member 102 and the second surface of the second member 112. The second resin 30 is arranged in a region other than between the first electrode 110 and the second electrode 114 facing each other. In the present embodiment, when viewed in the facing direction of the electrodes (the D1 direction), the second resin 30 is arranged in a region other than the second electrode 114 of the second surface. That is, in the second surface of the second member 112, the second resin 30 is arranged between and around the plurality of second electrodes 114 adjacent in the surface direction (the D2-D3 surface direction). In the second surface of the second member 112, the conductive particles 10 and the first resin 20 arranged in the second electrode 114 are surrounded by the second resin 30 in the surface direction (the D2-D3 surface direction). That is, in the second surface of the second member 112, the plurality of conductive particles 10 are surrounded by the first resin 20, and the first resin 20 is surrounded by the second resin 30. The first resin 20 and the second resin 30 are insulating resins. Therefore, the connection structure 100 has insulating properties in the plane direction (D2-D3 plane direction). By configuring in this way, the second resin 30 can reliably insulate between the plurality of first electrodes 110 adjacent to each other in the plane direction (D2-D3 plane direction), between the plurality of second electrodes 114 adjacent to each other in the plane direction (D2-D3 plane direction), and between the first electrode 110 and the second electrode 114 that are not facing each other.
[0046] The first resin 20 and the second resin 30 are arranged between the region other than the first electrode 110 of the first surface and the region other than the second electrode 114 of the second surface. The first resin 20 is arranged in contact with the first surface, and the second resin 30 is arranged in contact with the region other than the second electrode 114 of the second surface. That is, the first resin 20 and the second resin 30 are in contact in the surface direction (D2-D3 surface direction) between the region other than the first electrode 110 of the first surface and the region other than the second electrode 114 of the second surface, and are stacked in the opposite direction of the electrodes (D1 direction).
[0047] The boundary between the first resin 20 and the second resin 30 can be confirmed by observing the cross section of the connection structure 100. Since the first resin 20 and the second resin 30 have different compositions, the boundary between the first resin 20 and the second resin 30 can also be determined by using a processing / observation device such as a focused ion beam processing and observation device (FIB), a scanning electron microscope (SEM), or a transmission electron microscope (TEM).
[0048] When the first composition 20' and the second composition 30' described below are difficult to dissolve in each other, the boundary between the first resin 20 and the second resin 30 can be confirmed as an interface. When the first composition 20' and the second composition 30' have similar compositions and the interface disappears in the following steps, it may be observed as a boundary layer in which the first resin 20 and the second resin 30 are mixed.
[0049] The first electronic element 101 may be, for example, a flat panel display such as a liquid crystal display, an organic EL display, or a plasma display, and the first member 102 may be, for example, an insulating substrate such as a glass substrate or a transparent film substrate. The first electrode 110 may be, for example, an external connection terminal provided on the display. The first electrode 110 and the terminal 104 may be formed of transparent conductive materials such as ITO (indium tin oxide) and IZO (indium zinc oxide), metals such as copper (Cu), aluminum (Al), molybdenum (Mo), and titanium (Ti), and alloys containing at least one of them (Mo-Ti alloy, etc.), and laminated structures of these materials (Mo / Cu laminated structure, Mo-Ti alloy / Cu laminated structure, Mo / Al laminated structure, Mo / Al / Mo laminated structure, Al / Ti laminated structure, etc.).
[0050] The second electronic element 111 may be a Si chip formed with an integrated circuit. In this case, the second electrode 114 is equivalent to an external connection terminal (pad) provided on the integrated circuit. The second member 112 is preferably a silicon substrate, a SiC substrate, a sapphire substrate, a plastic substrate, etc. The second electrode 114 is preferably formed by gold (Au) or gold plating on the surface of copper (Cu). When the second electronic element 111 is, for example, a flexible printed substrate, the second member 112 is preferably an insulating polymer film such as polyimide or para-polyamide. The second electrode 114 is, for example, equivalent to an external connection terminal provided on a flexible printed substrate, generally formed of copper (Cu), and gold-plated on the surface.
[0051] There is no particular limitation on the size of the first electrode 110 and the second electrode 114 observed in the opposite direction (D1 direction). There is no particular limitation on the distance between the plurality of first electrodes 110 adjacent to each other in the surface direction (D2-D3 surface direction) (the distance between the plurality of second electrodes 114 adjacent to each other in the surface direction), for example, it can be 5 μm or more. By adopting such a structure, the first electrode 110 and the second electrode 114 can be electrically connected without damaging the insulation. In the present embodiment, the first electrode 110 and the second electrode 114 are arranged in a row at one end of the first electronic component 101 and the second electronic component 111 with their short sides arranged side by side. However, this is not limited to this, and the first electrode 110 and the second electrode 114 can also be arranged in multiple columns, or in a zigzag lattice shape.
[0052] The conductive particles 10 included in the connection structure 100 may be oblate spherical. The diameter (major diameter) of the conductive particles 10 observed in the direction opposite to the electrodes (D1 direction) is in the range of 2 μm to 10 μm. The conductive particles 10 may be originally spherical with the above-mentioned major diameter as the diameter, and may be deformed to be flat in the direction opposite to the electrodes (D1 direction) in the range of 10% to 40% relative to 100% of the major diameter by the following connection structure manufacturing method. The diameter (major diameter) and the pressure deformation amount of the conductive particles 10 may be appropriately selected within the above range according to the types of the first electronic component 101, the second electronic component 111, and the manufacturing methods of each connection structure. In this embodiment, as Figure 1 As shown in (D), the conductive particles 10 are in the form of perfect spheres. However, this is not limiting. Figure 1 As shown in (E), it is spherical and has a plurality of protrusions on the surface (wolf-tooth spherical shape). By having fine protrusions on the surface of the spherical shape like this, it is more preferable because, for example, the natural oxide film in the connection area can be broken.
[0053] The material of the conductive particles 10 is not particularly limited, and can be appropriately selected from known conductive particles and used. Figure 1 As shown in (D) and (E), metal-coated particles may be used, and the metal-coated particles have coating layers 10b and 10c that coat a particle core 10a obtained by coating a high-hardness resin material with a rubber-like elastic resin or a high-hardness inorganic material with a rubber-like inorganic elastic body with a metal such as nickel (Ni), copper (Cu), and gold (Au). For the metal coating, for example, a Ni / Cu stacked structure, a Ni / Au stacked structure, or a Cu / Au stacked structure may be formed by a drum sputtering method, a metal nanoparticle plating method, an electroless plating method, an ultrasonic plating method, or the like.
[0054] The first resin 20 and the second resin 30 are formed by curing the first composition 20' and the second composition 30' containing different materials. There is no particular limitation on the materials of the first composition 20' and the second composition 30', and they can be appropriately selected and used from known curable resin materials. In the present embodiment, the curable resin materials of the first composition 20' and the second composition 30' both contain free radical polymerizable resins. As free radical polymerizable resin materials, (meth) acrylic monomers or (meth) acrylate oligomers are preferred, and ester-type bonds are more preferred. (Meth) acrylic oligomers have at least one or more (meth) acryloyl groups, for example, epoxy acrylate, acrylic urethane, polyester acrylate, polybutadiene acrylate, polyol acrylate, polyether acrylate, silicone resin acrylate, melamine acrylate, etc. can be used. It can be any of monofunctional and multifunctional, but it is more preferred to contain multifunctional monomers or oligomers. The curable resin material can be composed of two or more selected from (meth)acrylate monomers and (meth)acrylate oligomers.
[0055] As the curable resin material of the second composition 30', a material with a low volume shrinkage during curing is particularly preferred. Therefore, the (meth) acrylic monomer compound may contain, for example, an amide hydroxymethyl structural part, or may contain a dendritic polymer or a hyperbranched polymer structural part. During photocuring, the (meth) acrylic monomer compound having an amide hydroxymethyl structural part polymerizes with each other as the carbon-carbon double bonds derived from (meth) acrylic acid, and the methylene-oxygen of the amide hydroxymethyl structural part is cut off. Therefore, the second composition 30' contains a (meth) acrylic monomer compound having at least one amide hydroxymethyl structural part composed of -CO-NH-CH2-O- in the molecule as a curing component, thereby being able to further suppress the volume shrinkage of the second resin 30 generated by curing the second composition 30', and being able to suppress the warping caused by the difference in bending rigidity between the first electronic component 101 and the second electronic component 111. By including a dendritic polymer or hyperbranched polymer structure having acryloyl groups arranged in the branches, the van der Waals distance between the branches is shorter than the van der Waals distance of a normal molecule. Therefore, the second composition 30' includes a dendritic polymer or hyperbranched polymer structure having acryloyl groups arranged as a curing component, so that the volume shrinkage of the second resin 30 caused by curing the second composition 30' can be further suppressed, and the warping caused by the difference in bending rigidity between the first electronic component 101 and the second electronic component 111 can be suppressed.
[0056] As the curable resin material of the second composition 30', it is preferred to use a fluorene-based acrylate. The second composition 30' may include an ene / thiol-based curable resin as a curing component, and the ene / thiol-based curable resin contains a compound having an ethylenically unsaturated double bond and a thiol compound, and at least one of these components may include a compound having a 9,9-diarylfluorene skeleton. As a 9,9-diarylfluorene compound, a 9,9-diarylfluorene compound having an ethylenically unsaturated bond and / or a 9,9-diarylfluorene compound having a mercapto group may also be included. As an ethylenically unsaturated compound, for example, 9,9-bis(4-acryloyloxyethoxyphenyl)fluorene (manufactured by Osaka Gas Chemical (Co., Ltd.), OGSOL EA-0200), phenoxyethyl acrylate (manufactured by Kyoeisha Chemical (Co., Ltd.), Light Acrylate POA) may also be used. As the thiol compound, for example, pentaerythritol tetrakis (3-mercaptobutyrate) (produced by Showa Denko Co., Ltd., Karenz MT PE1) can be used. Since the second composition 30' contains such a curable resin material, the volume shrinkage of the second resin 30 caused by curing the second composition 30' can be further suppressed, and the warping caused by the difference in bending rigidity between the first electronic component 101 and the second electronic component 111 can be suppressed.
[0057] As the curable resin material of the second composition 30', a material obtained by treating an ene / thiol curable resin with an oxidizing compound may also be used. The ene / thiol curable resin includes: an ene compound having two or more functional groups selected from the group consisting of allyl ether groups, vinyl ether groups, acrylate groups and methacrylate groups in the molecule, or a mixture of two or more of the above ene compounds; and a thiol compound having two or more thiol groups in one molecule. As a compound having two or more mercapto groups in one molecule, esters of mercaptocarboxylic acid and polyols, aliphatic polythiols, aromatic polythiols, and other polythiols may be included, and one or more of them may be used. For the oxidizing compound treatment, it is preferably carried out using a gas with oxidizing ability. The gas with oxidizing ability is a compound that has the properties of a gas under the temperature and pressure conditions of the oxidizing compound treatment and has oxidizing ability. As the gas with oxidizing ability, air, oxygen, ozone, etc. may be used, and a mixed gas containing part of them may also be used. By treating the photocurable resin material with an oxidizing compound, the second composition 30' can improve its stability over time.
[0058] The materials of the first composition 20' and the second composition 30' also include a photocuring initiating component. The photocuring initiating component can be any compound that is a photoradical initiator and generates free radicals by irradiating ultraviolet rays or visible light. As ultraviolet free radical initiators, for example, acetophenone initiators, benzoin ether initiators, benzophenone initiators, α-diketone initiators, and thioxanthone initiators can be used. As visible light free radical initiators, for example, camphorquinone compounds and acylphosphine oxide compounds can be used. In addition, it can also be a component that is classified as an ultraviolet free radical initiator but can be used together with a sensitizer to initiate visible light free radicals. Sensitizers can be used appropriately as needed. As sensitizers, known compounds can be used, for example, amine compounds and (meth) acrylates of alkanolamines can be used. Multiple photocuring initiating components and sensitizers can be used together. For example, ultraviolet free radical initiators and visible light free radical initiators can be used together to expand the wavelength region that can be cured. The photocuring initiating component is more preferably a photo-radical initiator that generates free radicals within a range of 300 nm to 500 nm in wavelength of irradiated light. The photocuring initiating component is formulated so that the curable resin material can be cured at room temperature within a light irradiation time of preferably about 3 seconds or less, more preferably 1 second or less. In addition, the curable resin material is also appropriately selected so that it can be cured at room temperature within such a time.
[0059] In the present embodiment, it is more preferred that the first composition 20' and the second composition 30' further include a shielding curing active compound, such as a chain transfer agent. The chain transfer agent transfers the free radicals generated by light irradiation to the shielding portion that the light does not directly reach. The chain transfer agent can, for example, use a compound containing at least one selected from a carbamate bond, a urea bond, or an isocyanate group, and at least one alkoxysilyl group. In the photocuring reaction using the above-mentioned chain transfer agent, a polyol having a hydroxyl group as an anion is produced as a by-product. The polyol causes an ester exchange reaction with the alkoxysilyl group contained in the chain transfer agent, thereby further curing. That is, by including a chain transfer agent, free radical curing and anion curing are caused simultaneously, and the shielding portion that the light does not directly reach can be cured.
[0060] By making the first composition 20' and the second composition 30' contain a shielding portion curable active compound, the first composition 20' and the second composition 30' can be reliably cured even under the conditions of the materials, connection method, etc. of the first electronic component 101, the second electronic component 111, the first electrode 110 and the second electrode 114, where the first composition 20' and the second composition 30' cannot be cured only by the action of the photocuring initiating component generated by light irradiation.
[0061] In the present embodiment, the material of the first composition 20' may further include an anaerobic curing initiating component. The anaerobic curing initiating component may use a known system including an organic peroxide and a curing accelerator. For example, the organic peroxide may use hydrogen peroxides, ketone peroxides, diacyl peroxides, peroxyesters, etc. As a curing accelerator, for example, o-benzoylsulfonyl imide (saccharin), hydrazine compounds, amine compounds, thiol compounds, etc. may be used. For the anaerobic curing initiating component and the curing accelerator, multiple types may also be used together.
[0062] In the present embodiment, the first composition 20' is surrounded by the first surface (including the first electrode 110), the second surface (including the second electrode 114), and the second composition 30'. Furthermore, the first composition 20' contacts the first electrode 110, the second electrode 114, and the conductive particles 10. When the first composition 20' contains an anaerobic curing initiating component, since the first electrode 110, the second electrode 114, and the conductive particles 10 contain a transition metal component, the peroxide is decomposed by the redox reaction of the curing accelerator and the transition metal ions, thereby initiating anaerobic curing of the first composition 20'.
[0063] By making the first composition 20' further include an anaerobic curing initiating component, the first composition 20' can be reliably cured even under conditions such as the materials and connection methods of the first electronic component 101, the second electronic component 111, the first electrode 110 and the second electrode 114, where the first composition 20' cannot be cured by the action of the photocuring initiating component generated by light irradiation alone.
[0064] In order to improve or change the properties such as fluidity, coating characteristics, preservation, curing characteristics, and physical properties after curing, additives can be appropriately used as needed. As additives, known compounds can be used, for example, silane coupling agents, diluents, modifiers, surfactants, storage stabilizers, defoamers, leveling agents, etc. can be listed, but are not limited to this. As silane coupling agents, for example, epoxy systems, amino systems, mercapto-sulfide systems, urea systems, etc. can be used, but are not particularly limited. By adding silane coupling agents, the adhesion on the interface of organic materials and inorganic materials is improved.
[0065] The viscosity of the first composition 20' is higher than the viscosity of the second composition 30'. The viscosity of the first composition 20' is 5×10 3 cP or more and 5×10 5 The viscosity of the second composition 30' is 2×10 3 cP or more and 2×10 5cP or less. As long as the difference between the viscosity of the first composition 20' and the viscosity of the second composition 30' is more than 2 times, it is sufficient. The viscosity of the first composition 20' and the second composition 30' can also be controlled by the degree of polymerization of the resin material contained in the first composition 20' and the second composition 30'. The viscosity of each composition can be appropriately selected from the above range according to the type of the first electronic component 101 and the second electronic component 111, the method for making the connection structure, the method for configuring the composition, etc. When the viscosity of the first composition 20' is less than 5×10 3 cP, the uniform dispersibility of the conductive particles 10 deteriorates, and sedimentation or aggregation is easily generated. By making the viscosity of the first composition 20' higher than the viscosity of the second composition 30', the flow of the conductive particles 10 mixed in the first composition 20' can be suppressed, and the conductive particles 10 can be efficiently arranged between the first electrode 110 and the second electrode 114. Therefore, the connection reliability between the first electrode 110 and the second electrode 114 can be ensured.
[0066] The first resin 20 and the second resin 30 are formed by curing the first composition 20' and the second composition 30'. The volume shrinkage of the first resin 20 generated by curing the first composition 20' and the volume shrinkage of the second resin 30 generated by curing the second composition 30' are preferably 4% or less, and more preferably 2% or less. When the volume shrinkage of the first resin 20 and the second resin 30 is greater than 4%, internal shrinkage stress is generated, and warping is easily generated due to the difference in bending rigidity between the first electronic component 101 and the second electronic component 111, thereby reducing the reliability of the physical connection between the first electronic component 101 and the second electronic component 111.
[0067] For the first resin 20, it is more preferred that the adhesion to conductive materials such as metal materials and metal oxide materials is high. For the first resin 20, it is preferred that the adhesion to the metal material forming the first electrode 110 and the second electrode 114 is high, for example, it is preferred that the adhesion to Au and ITO is high. For the second resin 30, it is more preferred that the adhesion to the resin material is high. For the second resin 30, it is preferred that the adhesion to the insulating film material forming the first surface of the first component 102 and the second surface of the second component 112 is high, for example, it is preferred that the adhesion to insulating materials such as polyimide, para-polyamide film, P-SiNx, glass is high. For the adhesion of the first resin 20, it is preferably in the range of 500N / m or more. For the adhesion of the second resin 30, it is preferably in the range of 700N / m or more. The adhesion, glass transition temperature and hardness of each resin can be appropriately selected according to the types of the first electronic component 101 and the second electronic component 111, the method for making the connection structure, etc. By selecting the first resin 20 and the second resin 30 according to the materials of the adherends, the bonding strength between the first surface of the first member 102 and the second surface of the second member 112 can be further improved. Therefore, the reliability of the physical connection between the first electronic component 101 and the second electronic component 111 can be improved.
[0068] [Method for producing a connected structure]
[0069] Next, use Figures 2 to 5 , a method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Figures 2 to 5 In the following, a method for forming the connection structure 100 is described in detail.
[0070] First, the first composition 20' is arranged on the first surface of the first member 102, and a plurality of conductive particles 10 are arranged on the upper surface of the first electrode 110. The plurality of conductive particles 10 are mixed with the first composition 20' and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, a pad printing method using a rubber head to transfer the printed matter is particularly preferred. Figures 2 to 5 A method of arranging the plurality of conductive particles 10 and the first composition 20 ′ will be described.
[0071] Figure 2 The step of arranging a mixture of a plurality of conductive particles 10 and a first composition 20 ′ on a plate 240 is shown. Figure 3 yes Figure 2In this embodiment, the plate 240 is, for example, a flat gravure plate. In this embodiment, the plate 240 has a recess 246 corresponding to the first electrode 110. However, the present invention is not limited thereto, and the recess 246 only needs to correspond to the region where the plurality of conductive particles 10 and the first composition 20' are arranged on the first surface of the first member 102.
[0072] In this embodiment, the mixture of the conductive particles 10 and the first composition 20' is arranged on the plate 240 using the scraper 250. However, the present invention is not limited thereto, and the mixture of the conductive particles 10 and the first composition 20' may be arranged on the plate 240 using a roller or the like. Figure 2 (A)~(C) and Figure 3 As shown in (A) to (C), the scraper 250 is moved from one end to the other end of the plate 240 in a state where the tip is separated from the upper surface 244 of the plate 240. When the diameter of the conductive particles 10 is set to Y μm, the gap between the tip of the scraper 250 and the upper surface 244 of the plate 240 can be appropriately set within a range of greater than 0 μm and less than Y μm. Since the distance of the gap is smaller than the diameter Y μm of the conductive particles 10, the conductive particles 10 are not arranged on the upper surface 244 of the plate 240, but the first composition 20' is arranged.
[0073] When the diameter of the conductive particles 10 is Y, the depth from the tip of the scraper 250 to the bottom surface 242 of the recess 246 can be appropriately selected within a range greater than Y μm. Since the depth from the tip of the scraper 250 to the bottom surface 242 of the recess 246 is greater than the diameter Y μm of the conductive particles 10, the conductive particles 10 are disposed in the recess 246 together with the first composition 20'.
[0074] When the distance from the front end of the scraper 250 to the bottom surface 242 of the recess 246 is less than Y μm, the front end of the scraper 250 is likely to contact the conductive particles 10, and the conductive particles 10 may not be filled or the filled conductive particles 10 may be damaged. When the distance between the front end of the scraper 250 and the upper surface 244 of the plate 240 is greater than Y μm, the conductive particles 10 may be arranged on the upper surface 244 of the plate 240.
[0075] like Figure 2 (A) to (C) and Figure 3 As shown in (A) to (C), the conductive particles 10 and the first composition 20' are arranged on the plate 240 by moving the scraper 250 from one end to the other end of the plate 240. In this embodiment, it is preferred that the scraper 250 is moved from one end to the other end of the plate 240 along the short side direction (D3 direction) of the recess 246. Thereby, the displacement of the conductive particles 10 arranged in one recess 246 can be suppressed.
[0076] The concentration of the conductive particles 10 mixed in the first composition 20' is preferably in a range of 20% by volume or more and 60% by volume or less relative to the total volume of the conductive particles 10 and the first composition 20'. If the mixing amount of the conductive particles 10 is less than 20% by volume, it is difficult to fill a sufficient amount of the conductive particles 10 in the recess 246. If the mixing amount of the conductive particles 10 is greater than 60% by volume, the workability is deteriorated, and it is difficult to fill the mixture of the conductive particles 10 and the first composition 20' in the recess 246. By placing the mixture of the conductive particles 10 and the first composition 20' using the scraper 250, the conductive particles 10 and the first composition 20' are filled in the recess 246 of the plate 240, and the first composition 20' is placed on the upper surface 244 of the plate 240.
[0077] Since the recess 246 has a depth within the above range, one conductive particle 10 can be held in the depth direction (D1 direction) of the recess 246. When viewed from the upper surface of the plate 240, the number of conductive particles 10 disposed in one recess 246 is preferably 7 / 400 μm. 2 More than 20 pieces / 400μm 2 By disposing in this way, in the step of transferring the mixture of the conductive particles 10 and the first composition 20 ′ to the pad described below, the conductive particles 10 and the first composition 20 ′ can be efficiently transferred to the pad.
[0078] It is preferable that the recesses 246 are spaced apart by 5 μm or more. If the recesses 246 are spaced apart by less than 5 μm, the wall separating the adjacent recesses 246 may be easily damaged, and the durability of the plate 240 may be reduced.
[0079] In the present embodiment, the shape of the recess 246 observed in the opposite direction of the electrodes (D1 direction) is the same rectangle as the first electrode 110 (or the second electrode 114). In addition, the recess 246 has the same shape in the depth direction. That is, the recess 246 has a shape obtained by cutting a rectangular parallelepiped from the plate 240. However, this is not limited to this, and the shape of the recess 246 can be any shape as long as the depth and area are within the above range. For example, it can also correspond to a complex shape.
[0080] The plate 240 may be, for example, a glass intaglio plate, a nickel plate intaglio plate, or a stainless steel plate intaglio plate, and may be subjected to plasma surface treatment using fluorine-based gas, nickel plating, or DLC (diamond-like carbon) treatment to improve the durability of the plate 240 as required.
[0081] Figure 42 shows a step of transferring a mixture of a plurality of conductive particles 10 and a first composition 20' from a plate 240 to a pad 230. Figure 4 As shown in (A) to (C), the first composition 20' disposed on the upper surface 244 of the plate 240, the conductive particles 10 filled in the concave portion 246 of the plate 240, and the first composition 20' are transferred to the glue head 230 by pushing the glue head 230 in a direction substantially perpendicular to the plate 240 and separating the glue head 230 in a direction substantially perpendicular to the plate 240. Since the viscosity of the first composition 20' is 5×10 3 cP or more and 5×10 5 Since the conductive particles 10 mixed in the first composition 20 ′ are within the range of cP or less, the conductive particles 10 can be held on the surface of the pad 230 .
[0082] The material of the pad 230 is preferably, for example, an elastic silicone resin. The shape of the pad 230 preferably has at least a convex structure. The shape of the pad 230 can be appropriately designed according to the shapes of the first electronic component 101 and the board 220 .
[0083] Figure 5 (A) to (B) show the steps of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the pad 230 to the first surface of the first member 102. Figure 5 As shown in (A) to (B), the mixture of the conductive particles 10 and the first composition 20' transferred to the glue head 230 is transferred to the first electrode 110 by pushing the glue head 230 in a direction substantially perpendicular to the first surface and separating the glue head 230 in a direction substantially perpendicular to the first surface. Here, the first composition 20' and the conductive particles 10 transferred from the concave portion 246 of the plate 240 are arranged in contact with the first electrode 110. That is, the first composition 20' is arranged on the first surface of the first member 102, and the conductive particles 10 are arranged on the upper surface of the first electrode 110. Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP above 5×10 5 Since the range of cP or less is 1.5 cP, the conductive particles 10 mixed in the first composition 20' can be held on the first electrode 110. By using this method, the conductive particles 10 and the first composition 20' can be reliably arranged in a predetermined region on the first electrode 110.
[0084] The first composition 20' and the conductive particles 10 transferred from the concave portion 246 of the plate 240 are arranged thicker on the first electrode 110 on the first member 102 in the direction facing the electrodes (the D1 direction) because they have the depth of the concave portion 246. On the other hand, the first composition 20' transferred from the upper surface 244 of the plate 240 does not have the depth of the concave portion 246, so it is arranged thinner in the direction facing the electrodes (the D1 direction) in the region other than the first electrode 110 on the first member 102. However, the present invention is not limited thereto, and the first composition 20' may not be transferred from the upper surface 244 of the plate 240 to the pad 230, and may not be transferred from the pad 230 to the region other than the first electrode 110 on the first member 102. On the first surface of the first member 102, the first composition 20' forms a convex-concave structure in the direction facing the electrodes (the D1 direction). On the first surface of the first member 102 , the conductive particles 10 form a protruding structure together with the first composition 20 ′.
[0085] Next, the second composition 30' is disposed on the first surface of the first member 102. Figure 5 As shown in (C), the second composition 30' is arranged in an area other than the first electrode 110 of the first surface. Here, the first composition 20' transferred from the upper surface 244 of the plate 240 is arranged in an area other than the first electrode 110 on the first surface. Therefore, the second composition 30' is arranged in an overlapping manner in contact with the first composition 20'. By arranging the second composition 30', the first composition 20' and the conductive particles 10 forming the convex-concave structure are buried on the first surface of the first member 102. That is, on the first surface of the first member 102, the first composition 20', the conductive particles 10 and the second composition 30' form a substantially flat structure. In other words, the second composition 30' is arranged on the first surface of the first member 102 in an area other than the area (convex structure) where a plurality of conductive particles 10 and the first composition 20' are arranged. The second composition 30' is arranged on the first surface of the first member 102 in an area (concave structure) where the first composition 20' is arranged. Although not shown, in this embodiment, the second composition 30' is arranged by pad printing in the same manner as the mixture of the conductive particles 10 and the first composition 20'. However, the method of arranging the second composition 30' is not limited thereto, and any existing method can be used as long as it can be applied to a region other than the region where the plurality of conductive particles 10 and the first composition 20' are arranged. For example, inkjet or dispensing, screen printing, etc. can be used.
[0086] The viscosity of the second composition 30' is 2×10 3 cP or more and 2×10 5The viscosity of the first composition 20' only needs to be higher than the viscosity of the second composition 30', and the difference in viscosity is at least 2 times. Thus, the flow of the conductive particles 10 mixed in the first composition 20' can be suppressed, so that the conductive particles 10 can be held on the first electrode 110.
[0087] Next, the second member 112 is mounted on the first surface of the first member 102. Figure 5 As shown in (D), the first surface of the first member 102 and the second surface of the second member 112 are arranged opposite to each other in such a manner that the corresponding plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposite to each other. The first member 102 and the second member 112 are pressed, and the first surface of the first member 102 and the second surface of the second member 112 are pushed in a direction substantially perpendicular to each surface. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20' and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because of its higher viscosity than the second composition 30'. The conductive particles 10 and the first composition 20 ′ disposed on the first electrode 110 are in contact with the second electrode 114 , and the second composition 30 ′ disposed in the area other than the first electrode 110 on the first surface is in contact with the area other than the second electrode 114 on the second surface.
[0088] like Figure 5 As shown in (E), the first member 102 and the second member 112 are further pressed, thereby pushing the first surface of the first member 102 and the second surface of the second member 112 in the substantially perpendicular direction of each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower parts of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10, the elastic force of the first composition 20' and the second composition 30'.
[0089] Here, the pressure is applied until the conductive particle 10 is deformed into an oblate spheroid due to the pressure from the first electrode 110 and the second electrode 114. The pressure deformation amount of the conductive particle 10 is controlled within a range of 10% or more and 40% or less relative to 100% of the major axis of the conductive particle 10. At this time, by applying stress between the first electrode 110, the conductive particle 10, and the second electrode 114, the first composition 20' between the first electrode 110 and the conductive particle 10, and between the second electrode 114 and the conductive particle 10 is excluded. In addition, even if a natural oxide film is formed on the first electrode 110, the conductive particle 10, or the second electrode 114 and the surface is insulated, the first electrode 110 and the second electrode 114 can be pressed and bonded with the conductive particle 10 sandwiched therebetween, thereby breaking through the natural oxide film and forming a conductive path. By deforming the conductive particles 10, the contact area between the first electrode 110 and the conductive particles 10 and the contact area between the second electrode 114 and the conductive particles 10 can be increased. By disposing the conductive particles 10 in this manner, the conductive particles 10 can electrically connect the first electrode 110 and the second electrode 114.
[0090] In a state where the first member 102 and the second member 112 are pressed, the connection structure 100 is irradiated with light. For the wavelength region, ultraviolet light and / or visible light region are preferred, and ultraviolet light is particularly preferred. The wavelength region of light can be appropriately selected according to the photocuring initiating components contained in the first composition 20' and the second composition 30'. The direction of light irradiation can be appropriately selected from the first electronic component 101 side or the second electronic component 111 side according to the wavelength region of light and the materials of the first member 102, the second member 112, etc. In addition, it is also preferred to irradiate from both sides, and irradiation from the side without a shield is also effective. The irradiation time of light can be appropriately selected according to the photocuring initiating components and curable resin materials contained in the first composition 20' and the second composition 30'. Generally speaking, it is preferably less than about 3 seconds, and more preferably less than about 1 second. In other words, the light irradiation intensity, photocuring initiating components, curable resin materials, etc. are appropriately selected in such a way that room temperature curing can be performed within such a time.
[0091] By light irradiation, most of the first composition 20' and the second composition 30' contained in the connection structure 100 are cured at room temperature. Then, there will be insufficient curing between the first electrode 110 and the second electrode 114 where the light does not fully reach. Therefore, for the material of the first composition 20', it is more preferred to include a shielding part curing active compound or an anaerobic curing initiating component. By including a shielding part curing active compound or an anaerobic curing initiating component, room temperature curing can also be promoted in the part where the light does not fully reach. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting this structure, the first surface of the first electronic component 101 can be physically connected to the second surface of the second electronic component 111.
[0092] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged on the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.
[0093] <Second embodiment>
[0094] The structure of the connection structure of this embodiment is the same as that of the connection structure of the first embodiment. The method for preparing the connection structure of this embodiment is the same as that of the connection structure of the first embodiment, except that the second composition 30' is arranged in the area other than the second electrode 114 of the second surface. The same description as that of the first embodiment is omitted, and only the parts different from the method for preparing the connection structure of the first embodiment are described here.
[0095] [Method for producing a connected structure]
[0096] use Figure 6 A method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Figure 6 In the following, a method for forming the connection structure 100 is described in detail.
[0097] First, the first composition 20' is arranged on the first surface of the first member 102, and a plurality of conductive particles 10 are arranged on the upper surface of the first electrode 110. The plurality of conductive particles 10 are mixed with the first composition 20' and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, a pad printing method using a pad to transfer the printed matter is particularly preferred. Since the area and method for arranging the mixture of the plurality of conductive particles 10 and the first composition 20' are the same as the method for preparing the connection structure of the first embodiment, they are omitted here.
[0098] Figure 6 (A) to (B) show the steps of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the pad 230 to the first surface of the first member 102. Figure 6 As shown in (A) to (B), the mixture of the conductive particles 10 and the first composition 20' transferred to the rubber head 230 is transferred to the first surface by pushing the rubber head 230 in a direction substantially perpendicular to the first surface and separating the rubber head 230 in a direction substantially perpendicular to the first surface. Here, the first composition 20' and the conductive particles 10 transferred from the concave portion 246 of the plate 240 are arranged in contact with the first electrode 110. That is, the first composition 20' is arranged on the first surface of the first member 102, and the conductive particles 10 are arranged on the upper surface of the first electrode 110. Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP above 5×10 5 Since the range of cP or less is 1.5 cP, the conductive particles 10 mixed in the first composition 20' can be held on the first electrode 110. By using this method, the conductive particles 10 and the first composition 20' can be reliably arranged in a predetermined region on the first electrode 110.
[0099] The first composition 20' and the conductive particles 10 transferred from the concave portion 246 of the plate 240 are arranged thicker on the first electrode 110 on the first member 102 in the direction facing the electrodes (the D1 direction) because they have the depth of the concave portion 246. On the other hand, the first composition 20' transferred from the upper surface 244 of the plate 240 does not have the depth of the concave portion 246, so it is arranged thinner in the direction facing the electrodes (the D1 direction) in the region other than the first electrode 110 on the first member 102. However, the present invention is not limited thereto, and the first composition 20' may not be transferred from the upper surface 244 of the plate 240 to the pad 230, and may not be transferred from the pad 230 to the region other than the first electrode 110 on the first member 102. On the first surface of the first member 102, the first composition 20' forms a convex-concave structure in the direction facing the electrodes (the D1 direction). On the first surface of the first member 102 , the conductive particles 10 form a protruding structure together with the first composition 20 ′.
[0100] Next, the second composition 30' is disposed on the second surface of the second member 112. Figure 6 As shown in (C) to (D), the second composition 30' is arranged in an area other than the second electrode 114 on the second surface of the second member 112. In other words, the second composition 30' is arranged on the second surface of the second member 112 in an area other than the area corresponding to the area where the plurality of conductive particles 10 and the first composition 20' are arranged. Although not shown, in the present embodiment, the second composition 30' is arranged using a pad printing method. However, it is not limited thereto, and as for the method of arranging the second composition 30', as long as it can be coated differently from the area other than the area where the plurality of conductive particles 10 and the first composition 20' are arranged, an existing method can be used. For example, inkjet or coating using a dispenser, screen printing, etc. can be used.
[0101] The viscosity of the second composition 30' is 2×10 3 cP above 2×10 5 This can suppress the flow of the second composition 30'.
[0102] Next, the second member 112 is mounted on the first surface of the first member 102. Figure 6As shown in (E), the first surface of the first member 102 and the second surface of the second member 112 are arranged opposite to each other in such a manner that the corresponding plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposite to each other. The first member 102 and the second member 112 are pressed, and the first surface of the first member 102 and the second surface of the second member 112 are pushed in a direction substantially perpendicular to each surface. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20' and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because of its higher viscosity than the second composition 30'. The conductive particles 10 and the first composition 20' disposed on the first electrode 110 are arranged in an overlapping manner so as to contact the second electrode 114, and the second composition 30' disposed in the area other than the second electrode 114 on the second surface contacts the first composition 20' disposed in the area other than the first electrode on the first surface. The second composition 30' disposed on the second surface of the second member 112 is disposed on the first surface of the first member 102 in which the first composition 20' and the conductive particles 10 form a convex-concave structure, so that the convex-concave structure is buried. That is, the first surface of the first member 102 and the second surface of the second member 112 are filled with the first composition 20', the conductive particles 10, and the second composition 30'. In other words, the second composition 30' disposed on the second surface of the second member 112 is disposed in an area other than the area (convex structure) where a plurality of conductive particles 10 and the first composition 20' are disposed on the first surface of the first member 102. The second composition 30 ′ disposed on the second surface of the second member 112 is disposed on the first surface of the first member 102 in the region (concave structure) where the first composition 20 ′ is disposed.
[0103] like Figure 6 As shown in (F), the first member 102 and the second member 112 are further pressed, thereby pushing the first surface of the first member 102 and the second surface of the second member 112 in the substantially perpendicular direction of each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower sides of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10, the elastic force of the first composition 20' and the second composition 30'. By adopting this structure, the first electrode 110 and the second electrode 114 can be electrically connected.
[0104] In a state where the first member 102 and the second member 112 are pressed, the connection structure 100 is irradiated with light to cure the first composition 20' and the second composition 30'. Since the method for curing the first composition 20' and the second composition 30' is the same as the method for making the connection structure of the first embodiment, it is omitted here. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting this structure, the first surface of the first electronic component 101 and the second surface of the second electronic component 111 can be physically connected.
[0105] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged on the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.
[0106] <Third embodiment>
[0107] The structure of the connection structure of the present embodiment is the same as that of the connection structure of the first embodiment, except that the stacking order of the first resin 20 and the second resin 30 between the region other than the first electrode 110 on the first surface and the region other than the second electrode 114 on the second surface is different. The method for preparing the connection structure of the present embodiment is the same as that of the connection structure of the first embodiment, except that the step of preparing the mixture of the plurality of conductive particles 10 and the first composition 20' and the step of preparing the second composition 30' are exchanged. The same description as that of the first embodiment is omitted, and only the parts different from the connection structure and the method for preparing the connection structure of the first embodiment are described here.
[0108] [Structure of the connection structure]
[0109] Figure 7 The structure of a connection structure according to one embodiment of the present invention is shown. Figure 7 (A) is a plan view of a connection structure according to one embodiment of the present invention. Figure 7 (B) Yes Figure 7 (A) D-D' cross-sectional view. Figure 7 (C) Yes Figure 7 (B) is an enlarged cross-sectional view of the conductive particles in the region E.
[0110] like Figure 7As shown in (A) and (B), the first electronic component 101 includes a terminal 104, a first insulating film 106, a second insulating film 108, and a first electrode 110 on the connection surface (first surface) of the first member 102. The second electronic component 111 is mounted on the connection surface (first surface) of the first electronic component 101. The second electronic component 111 includes a second electrode 114 on the connection surface (second surface) of the second member 112. The first surface of the first electronic component 101 and the second surface of the second electronic component 111 are arranged to face each other. The connection structure 100a is responsible for the physical connection between the first electronic component 101 and the second electronic component 111, and the electrical connection between the first electrode 110 and the second electrode 114. The connection structure 100a includes the first surface of the first member 102, the first electrode 110, the second surface of the second member 112, the second electrode 114, the conductive particles 10, the first resin 20, and the second resin 30.
[0111] A plurality of first electrodes 110 and a plurality of second electrodes 114 are arranged opposite to each other. A plurality of conductive particles 10 and a first resin 20 are arranged between the first and second electrodes 110, 114. A plurality of conductive particles 10 are arranged in a plane direction (D2-D3 plane direction) between the first and second electrodes 110, 114. One conductive particle 10 is arranged in a direction (D1 direction) facing the first and second electrodes 110, 114 between the first and second electrodes 110, 114. Each conductive particle 10 contacts the first and second electrodes 110, 114. Figure 7As shown in (C), the conductive particle 10 is deformed by pressure in the direction of the electrodes facing each other (D1 direction) between the first electrode 110 and the second electrode 114 by the following method for producing a connection structure. That is, the distance between the first electrode 110 and the second electrode 114 in the direction of the electrodes facing each other (D1 direction) is approximately the same as the height of the conductive particle 10 in the direction of the electrodes facing each other (D1 direction). The height of the conductive particle 10 in the direction of the electrodes facing each other (D1 direction) is deformed by pressure by about 10% to 40%. By applying stress between the first electrode 110, the conductive particle 10, and the second electrode 114, the first resin 20 is excluded from the contact portion between the first electrode 110 and the conductive particle 10, and the contact portion between the second electrode 114 and the conductive particle 10. Furthermore, even if a natural oxide film is formed on the first electrode 110, the conductive particles 10, or the second electrode 114 and the surface is insulated, the natural oxide film can be broken and a conductive path can be formed by pressing the first electrode 110 and the second electrode 114 with the conductive particles 10 interposed therebetween. Furthermore, by deforming the conductive particles 10, the contact area between the first electrode 110 and the conductive particles 10 and the contact area between the second electrode 114 and the conductive particles 10 can be increased. By configuring in this way, the conductive particles 10 can electrically connect the first electrode 110 and the second electrode 114.
[0112] A plurality of conductive particles 10 are dispersed in the first resin 20 between the first electrode 110 and the second electrode 114. Each conductive particle 10 is surrounded by the first resin 20 in the surface direction (D2-D3 surface direction) between the first electrode 110 and the second electrode 114. The first resin 20 is an insulating resin. Therefore, the connection structure 100a has insulating properties in the surface direction (D2-D3 surface direction). However, a plurality of conductive particles 10 arranged between the first electrode 110 and the second electrode 114 facing each other and adjacent in the surface direction (D2-D3 surface direction) may also contact each other. When the conductive particles 10 adjacent in the surface direction (D2-D3 surface direction) contact each other, the adjacent conductive particles 10 are also electrically connected to each other. By configuring in this way, the conductive particles 10 can further reliably electrically connect the first electrode 110 and the second electrode 114 facing each other. The distance between adjacent conductive particles 10 can be appropriately controlled by adjusting the concentration of the conductive particles 10 mixed in the first composition 20 ′ described below.
[0113] In the present embodiment, when observed in the opposing direction of the electrodes (D1 direction), the first resin 20 is also arranged in the region other than the second electrode 114 of the second surface. When observed in the opposing direction of the electrodes (D1 direction), the first resin 20 is also arranged between and around the plurality of second electrodes 114 of the second surface. On the other hand, when observed in the opposing direction of the electrodes (D1 direction), the first resin 20 is not arranged at the end of the second surface. At this time, when observed in the opposing direction of the electrodes (D1 direction), the conductive particles 10 are not arranged in the region other than the first electrode 110 of the first surface (the second electrode 114 of the second surface). That is, the conductive particles 10 are arranged on the first electrode 110 (or the second electrode 114).
[0114] The second resin 30 is further arranged between the first surface of the first member 102 and the second surface of the second member 112. The second resin 30 is arranged in a region other than between the first electrode 110 and the second electrode 114 facing each other. In the present embodiment, when viewed in the facing direction of the electrodes (the D1 direction), the second resin 30 is arranged in a region other than the first electrode 110 of the first surface. That is, in the first surface of the first member 102, the second resin 30 is arranged between and around the plurality of first electrodes 110 adjacent in the surface direction (the D2-D3 surface direction). In the first surface of the first member 102, the conductive particles 10 and the first resin 20 arranged in the first electrode 110 are surrounded by the second resin 30 in the surface direction (the D2-D3 surface direction). That is, in the first surface of the first member 102, the plurality of conductive particles 10 are surrounded by the first resin 20, and the first resin 20 is surrounded by the second resin 30. The first resin 20 and the second resin 30 are insulating resins. Therefore, the connection structure 100a has insulating properties in the plane direction (D2-D3 plane direction). By configuring in this way, the second resin 30 can reliably insulate between the plurality of first electrodes 110 adjacent to each other in the plane direction (D2-D3 plane direction), between the plurality of second electrodes 114 adjacent to each other in the plane direction (D2-D3 plane direction), and between the first electrode 110 and the second electrode 114 that are not facing each other.
[0115] The first resin 20 and the second resin 30 are arranged between the region other than the first electrode 110 of the first surface and the region other than the second electrode 114 of the second surface. The first resin 20 is arranged in such a manner that the second electrode 114 is in contact with the region other than the first electrode 110 of the first surface, and the second resin 30 is in contact with the region other than the first electrode 110 of the first surface. That is, the first resin 20 and the second resin 30 are in contact in the surface direction (D2-D3 surface direction) between the region other than the first electrode 110 of the first surface and the region other than the second electrode 114 of the second surface, and are stacked in the direction of the electrodes facing each other (D1 direction).
[0116] [Method for producing a connected structure]
[0117] use Figure 8 A method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Figure 8 In the following, a method for forming the connection structure 100a is described in detail.
[0118] First, the second composition 30 is disposed on the first surface of the first member 102. Figure 8 As shown in (A) to (B), the second composition 30' is arranged in an area other than the first electrode 110 on the first surface of the first member 102. In other words, the second composition 30' is arranged on the first surface of the first member 102 in an area other than the area where the plurality of conductive particles 10 and the first composition 20' are arranged. Although not shown, in this embodiment, the second composition 30' is arranged using a pad printing method. However, it is not limited thereto, and as for the method of arranging the second composition 30', as long as it can be coated differently from the area other than the area where the plurality of conductive particles 10 and the first composition 20' are arranged, an existing method can be used. For example, inkjet or coating using a dispenser, screen printing, etc. can be used.
[0119] The viscosity of the second composition 30' is 2×10 3 cP above 2×10 5 This can suppress the flow of the second composition 30'.
[0120] Next, the first composition 20' is arranged on the first surface of the first member 102, and a plurality of conductive particles 10 are arranged on the upper surface of the first electrode 110. The plurality of conductive particles 10 are mixed with the first composition 20' and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, a pad printing method using a pad to transfer the printed matter is particularly preferred. Since the area and method for arranging the mixture of the plurality of conductive particles 10 and the first composition 20' are the same as the method for preparing the connection structure of the first embodiment, they are omitted here.
[0121] Figure 8 (C) to (D) show the steps of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the pad 230 to the first surface of the first member 102 by pad printing. Figure 8As shown in (C) to (D), the mixture of the conductive particles 10 and the first composition 20' transferred to the rubber head 230 is transferred to the first surface by pushing the rubber head 230 in a direction substantially perpendicular to the first surface and separating the rubber head 230 in a direction substantially perpendicular to the first surface. Here, the first composition 20' and the conductive particles 10 transferred from the concave portion 246 of the plate 240 are arranged in contact with the first electrode 110. That is, the first composition 20' is arranged on the first surface of the first member 102, and the conductive particles 10 are arranged on the upper surface of the first electrode 110.
[0122] The first composition 20' and the conductive particles 10 transferred from the recessed portion 246 of the plate 240 are arranged thicker on the first electrode 110 on the first member 102 in the direction facing the electrodes (the D1 direction) because they have the depth of the recessed portion 246. On the other hand, the first composition 20' transferred from the upper surface 244 of the plate 240 does not have the depth of the recessed portion 246, so it is arranged thinner in the direction facing the electrodes (the D1 direction) in the region other than the first electrode 110 on the first member 102. However, this is not limited to this, and the first composition 20' may not be transferred from the upper surface 244 of the plate 240 to the pad 230, and may not be transferred from the pad 230 to the region other than the first electrode 110 on the first member 102. Here, the second composition 30' is arranged in the region other than the first electrode 110 on the first surface. Therefore, the first composition 20' transferred from the upper surface 244 of the plate 240 is arranged in an overlapping manner so as to contact with the second composition 30'. In other words, the first composition 20' and the conductive particles 10 transferred from the concave portions 246 of the plate 240 are arranged on the first surface of the first member 102 in an area other than the area where the second composition 30' is arranged. By arranging the first composition 20' and the conductive particles 10 on the first surface of the first member 102 where the second composition 30' is arranged, the first composition 20', the conductive particles 10, and the second composition 30' form a substantially flat structure on the first surface of the first member 102.
[0123] Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP above 5×10 5 Since the range of cP or less is 1.5 cP, the conductive particles 10 mixed in the first composition 20' can be held on the first electrode 110. By using this method, the conductive particles 10 and the first composition 20' can be reliably arranged in a predetermined area on the first electrode 110.
[0124] Next, the second electronic component 111 is mounted on the first surface of the first electronic component 101. Figure 8As shown in (E), the first surface of the first member 102 and the second surface of the second member 112 are arranged opposite to each other in such a manner that the plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposite to each other. The first member 102 and the second member 112 are pressed, and the first surface of the first member 102 and the second surface of the second member 112 are pushed in a direction substantially perpendicular to each surface. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20' and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because the viscosity is higher than that of the second composition 30'. The conductive particles 10 and the first composition 20 ′ disposed on the first electrode 110 are in contact with the second electrode 114 , and the first composition 20 ′ disposed on the first surface other than the first electrode 110 is in contact with the second surface other than the second electrode 114 .
[0125] like Figure 8 As shown in (F), the first member 102 and the second member 112 are further pressed, thereby pushing the first surface of the first member 102 and the second surface of the second member 112 in the substantially perpendicular direction of each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower sides of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10, the elastic force of the first composition 20' and the second composition 30'.
[0126] While the first member 102 and the second member 112 are pressed, the connection structure 100a is irradiated with light to cure the first composition 20' and the second composition 30'. Since the method for curing the first composition 20' and the second composition 30' is the same as the method for making the connection structure of the first embodiment, it is omitted here. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting this structure, the first surface of the first electronic component 101 and the second surface of the second electronic component 111 can be physically connected.
[0127] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged on the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.
[0128] <Fourth embodiment>
[0129] The structure of the connection structure of this embodiment is the same as that of the connection structure of the third embodiment. The method for producing the connection structure of this embodiment is the same as that of the first embodiment, except that the second composition 30' is arranged in the area other than the first electrode 110 of the first member 102, and the plurality of conductive particles 10 and the first composition 20' are arranged on the second electrode 114 of the second member 112. The same description as that of the first embodiment is omitted, and only the parts different from the method for producing the connection structure of the first embodiment are described here.
[0130] [Method for producing a connected structure]
[0131] use Fig. 9 A method for manufacturing a connection structure according to an embodiment of the present invention is described. In addition, in this embodiment, since the existing first electronic component 101 and second electronic component 111 can be used, their description is omitted. Fig. 9 In the following, a method for forming the connection structure 100a is described in detail.
[0132] First, the second composition 30' is disposed on the first surface of the first member 102. Fig. 9 As shown in (A) to (B), the second composition 30' is arranged in an area other than the first electrode 110 on the first surface of the first member 102. In other words, the second composition 30' is arranged on the first surface of the first member 102 in an area other than the area corresponding to the area where the plurality of conductive particles 10 and the first composition 20' are arranged. Although illustrated, in the present embodiment, the second composition 30' is arranged using a pad printing method. However, it is not limited thereto, and as for the method of arranging the second composition 30', as long as it can be coated differently from the area other than the area where the plurality of conductive particles 10 and the first composition 20' are arranged, an existing method can be used. For example, inkjet or coating using a dispenser, screen printing, etc. can be used.
[0133] The viscosity of the second composition 30' is 2×10 3 cP above 2×10 5 This can suppress the flow of the second composition 30'.
[0134] Next, the first composition 20' is arranged on the second surface of the second member 112, and a plurality of conductive particles 10 are arranged on the upper surface of the second electrode 114. The plurality of conductive particles 10 are mixed with the first composition 20' and arranged using an offset printing method. Since the mixture of the conductive particles 10 and the first composition 20' contains the conductive particles 10, a pad printing method using a pad to transfer the printed matter is particularly preferred. Since the area and method for arranging the mixture of the plurality of conductive particles 10 and the first composition 20' are the same as the method for preparing the connection structure of the first embodiment, they are omitted here.
[0135] Fig. 9 (C) to (D) show the steps of transferring the mixture of the plurality of conductive particles 10 and the first composition 20' from the pad 230 to the second surface of the second member 112 by pad printing. Fig. 9 As shown in (C) to (D), the mixture of the conductive particles 10 and the first composition 20' transferred to the rubber head 230 is transferred to the second surface by pushing the rubber head 230 in a direction substantially perpendicular to the second surface and separating the rubber head 230 in a direction substantially perpendicular to the second surface. Here, the first composition 20' transferred from the concave portion 246 of the plate 240 and the conductive particles 10 are arranged in contact with the second electrode 114. That is, the first composition 20' is arranged on the second surface of the second member 112, and the conductive particles 10 are arranged on the upper surface of the second electrode 114. Since the viscosity of the curable resin material of the first composition 20' is 5×10 3 cP above 5×10 5 Since the range of cP or less is 0.1, the conductive particles 10 mixed in the first composition 20' can be held on the second electrode 114. By using this method, the conductive particles 10 and the first composition 20' can be reliably arranged in a predetermined region on the second electrode 114.
[0136] The first composition 20' and the conductive particles 10 transferred from the concave portion 246 of the plate 240 are arranged thicker on the second electrode 114 on the second member 112 in the direction facing the electrodes (the D1 direction) because they have the depth of the concave portion 246. On the other hand, the first composition 20' transferred from the upper surface 244 of the plate 240 does not have the depth of the concave portion 246, so it is arranged thinner in the direction facing the electrodes (the D1 direction) in the region other than the second electrode 114 on the second member 112. However, the present invention is not limited thereto, and the first composition 20' may not be transferred from the upper surface 244 of the plate 240 to the pad 230, and may not be transferred from the pad 230 to the region other than the second electrode 114 on the second member 112. That is, on the second surface of the second member 112, the first composition 20' forms a convex-concave structure in the direction facing the electrodes (the D1 direction). On the second surface of the second member 112 , the conductive particles 10 form a protruding structure together with the first composition 20 ′.
[0137] Next, the second electronic component 111 is mounted on the first surface of the first electronic component 101. Fig. 9As shown in (E), the first surface of the first member 102 and the second surface of the second member 112 are arranged opposite to each other in such a manner that the plurality of first electrodes 110 and the plurality of second electrodes 114 are respectively opposite to each other. The first member 102 and the second member 112 are pressed, and the first surface of the first member 102 and the second surface of the second member 112 are pushed in a direction substantially perpendicular to each surface. The first surface of the first member 102 and the second surface of the second member 112 are pressed against the conductive particles 10, the first composition 20' and the second composition 30'. At this time, the first composition 20' arranged on the first electrode 110 is held on the first electrode 110 together with the conductive particles 10 because the viscosity is higher than that of the second composition 30'. The conductive particles 10 and the first composition 20' arranged on the second electrode 114 are arranged in an overlapping manner in such a manner that "the conductive particles 10 and the first composition 20' arranged on the second electrode 114 are in contact with the first electrode 110, and the second composition 30' arranged in the area other than the first electrode 110 on the first surface is in contact with the first composition 20' arranged in the area other than the second electrode 114 on the second surface". The convex-concave structure is buried by arranging the first composition 20' and the conductive particles 10 forming the convex-concave structure on the second surface of the second member 112 on the first surface of the first member 102 on which the second composition 30' is arranged. That is, the first surface of the first member 102 and the second surface of the second member 112 are filled with the first composition 20', the conductive particles 10 and the second composition 30'. In other words, the plurality of conductive particles 10 and the first composition 20' (convex structure) arranged on the second surface of the second member 112 are arranged on the first surface of the first member 102 in an area other than the area on which the second composition 30' is arranged. The first composition 20 ′ (concave structure) disposed on the second surface of the second member 112 is disposed on the first surface of the first member 102 in the region where the second composition 30 ′ is disposed.
[0138] like Fig. 9 As shown in (F), the first member 102 and the second member 112 are further pressed, thereby pushing the first surface of the first member 102 and the second surface of the second member 112 in the substantially perpendicular direction of each surface. At this time, sufficient pressure is applied so that the first electrode 110 and the second electrode 114 facing each other contact the upper and lower parts of one conductive particle 10. The pressure for pushing the first surface of the first member 102 and the second surface of the second member 112 can be appropriately adjusted according to the repulsive force of the conductive particle 10, the elastic force of the first composition 20' and the second composition 30'.
[0139] In a state where the first member 102 and the second member 112 are pressed, the connection structure 100a is irradiated with light to cure the first composition 20' and the second composition 30'. Since the method for curing the first composition 20' and the second composition 30' is the same as the method for making the connection structure of the first embodiment, it is omitted here. By curing the first composition 20' and the second composition 30', the first resin 20 and the second resin 30 are formed. By adopting this structure, the first surface of the first electronic component 101 and the second surface of the second electronic component 111 can be physically connected.
[0140] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the electrodes facing each other and suppress the short circuit between adjacent connection electrodes even if the electrodes arranged on the electronic element are highly refined and highly dense by a simple process. Furthermore, since a heat curing connection method is not used, the electrodes of the upper and lower substrates with different thermal expansion coefficients can be connected to each other with high precision.
[0141] According to this embodiment, a method for manufacturing a connection structure and a connection structure can be provided, which can ensure the conductivity between the opposing electrodes and suppress the short circuit between adjacent connection electrodes through a simple process even if the electrodes arranged on the electronic components are highly refined and highly dense.
[0142] The present invention is not limited to the above-described embodiments, and can be appropriately modified within the scope of the gist. In addition, the various embodiments can be appropriately combined.
[0143] [Example 1]
[0144] Fig.10 This is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.10 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 1 of the present invention. Fig.10 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure of Example 1 of the present invention. The parameters of the connection structure of Example 1 are as follows.
[0145] Width (short side) of first electrode 110 (A1) = 9 μm
[0146] Distance between first electrodes 110 (B1) = 6 μm
[0147] · Span of the first electrode 110 (A1+B1=C1)=15 μm
[0148] Length (long side) of first electrode 110 (D1) = 105 μm
[0149] Area of the first electrode 110 (A1×D1)=945 μm 2
[0150] The number of conductive particles 10 arranged per one electrode = 19 particles.
[0151] [Example 2]
[0152] Fig.11 This is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.11 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 2 of the present invention. Fig.11 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure of Example 2 of the present invention. The parameters of the connection structure of Example 2 are as follows.
[0153] Width (short side) of first electrode 110 (A2) = 9 μm
[0154] Distance between first electrodes 110 (B2) = 6 μm
[0155] · Span of the first electrode 110 (A2+B2=C2)=15 μm
[0156] Length (long side) of first electrode 110 (D2) = 105 μm
[0157] The area of the first electrode 110 (A2×D2)=945 μm 2
[0158] The number of conductive particles 10 arranged per electrode = 26 particles.
[0159] [Example 3]
[0160] Fig.12 This is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.12 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 3 of the present invention. Fig.12 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure of Example 3 of the present invention. The parameters of the connection structure of Example 3 are as follows.
[0161] Width (short side) of first electrode 110 (A3) = 10 μm
[0162] Distance between first electrodes 110 (B3) = 18 μm
[0163] · Span of the first electrode 110 (A3+B3=C3)=28 μm
[0164] Length of one region where the conductive particles 10 and the first resin 20 are arranged (D3) = 10 μm
[0165] The distance between the regions where the conductive particles 10 and the first resin 20 are arranged (E3) = 7 μm
[0166] · Length (long side) of first electrode 110 (F3) = 44 μm
[0167] Area of the first electrode 110 (A3×F3)=440 μm 2
[0168] · Area of one region where the conductive particles 10 and the first resin 20 are arranged = 100 μm 2
[0169] The number of regions where the conductive particles 10 and the first resin 20 are arranged per electrode = 3
[0170] Total area of the region where the conductive particles 10 and the first resin 20 are arranged per electrode = 300 μm 2
[0171] The number of conductive particles 10 arranged per region where the conductive particles 10 and the first resin 20 are arranged = 6
[0172] The number of conductive particles 10 arranged per electrode = 18 particles.
[0173] [Example 4]
[0174] Fig.13 This is a diagram showing an example of a connection structure according to an embodiment of the present invention. Fig.13 (A) is a diagram showing an arrangement pattern of conductive particles 10 and a first resin 20 in a connection structure according to Example 4 of the present invention. Fig.13 (B) is a diagram showing an arrangement pattern of the first resin 20 and the second resin 30 of the connection structure of Example 4 of the present invention. The parameters of the connection structure of Example 4 are as follows.
[0175] Width (short side) of first electrode 110 (A4) = 8 μm
[0176] Distance between first electrodes 110 (B4) = 9 μm
[0177] · Span of the first electrode 110 (A4+B4=C4) = 17 μm
[0178] · Length (long side) of first electrode 110 (D4) = 40 μm
[0179] Area of the first electrode 110 (A4×D4)=320 μm 2
[0180] The number of conductive particles 10 disposed per first electrode 110 = 12 particles.
[0181] As shown in Examples 1 to 4, according to one embodiment of the present invention, even if the electrodes arranged on the electronic component are highly refined and highly dense, the conductivity between the opposing electrodes can be ensured through a simple process and the short circuit between adjacent electrodes can be suppressed.
[0182] (Description of the label)
[0183] 10···conductive particles, 20···first resin, 20'···first composition, 30···second resin, 30'···second composition, 100, 100a, 100b, 100c···connected structure, 101···first electronic component, 102···first member, 104···terminal, 106···first insulating film, 108···second insulating film, 110···first electrode, 111···second electronic component, 112···second member, 114···second electrode, 250···scraper, 240···plate, 246···recess, 230···rubber head.
Claims
1. A method for manufacturing a connection structure, comprising the following steps: Disposing a first composition on a first surface of a first member on which a first electrode is disposed, and disposing conductive particles on the first electrode; Disposing a second composition in an area other than the first electrode on the first surface so as to overlap with the first composition; The first surface and the second surface of the second member provided with the second electrode are arranged facing each other in such a manner that "the first composition and the conductive particles are in contact with the second electrode, and the second composition is in contact with the area other than the second electrode on the second surface"; pressing the first member and the second member; and The first composition and the second composition are cured.
2. A method for manufacturing a connection structure, comprising the following steps: Disposing a first composition on a first surface of a first member on which a first electrode is disposed, and disposing conductive particles on the first electrode; disposing a second composition in a region other than the second electrode disposed on the second surface of the second member; The first surface and the second surface are arranged facing each other in such a manner that "the first composition and the conductive particles are in contact with the second electrode, and the second composition overlaps the first composition in the area other than the first electrode of the first surface"; pressing the first member and the second member; and The first composition and the second composition are cured.
3. A method for manufacturing a connection structure, comprising the following steps: disposing a second composition in a region other than the first electrode disposed on the first surface of the first member; Disposing the first composition on the first surface so as to overlap with the second composition, and disposing conductive particles on the first electrode; The first surface and the second surface of the second member provided with the second electrode are arranged opposite to each other in a manner that "the conductive particles are in contact with the second electrode, and the first composition is in contact with the second surface"; pressing the first member and the second member; and The first composition and the second composition are cured.
4. A method for manufacturing a connection structure, comprising the following steps: disposing a second composition in a region other than the first electrode disposed on the first surface of the first member; The first composition is disposed on the second surface of the second member on which the second electrode is disposed, and conductive particles are disposed on the second electrode; The first surface and the second surface are arranged facing each other in such a manner that "the first composition and the conductive particles are in contact with the first electrode, and the second composition overlaps the first composition in the area other than the second electrode of the second surface"; pressing the first member and the second member; and The first composition and the second composition are cured.
5. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition is arranged using an offset printing method, and the conductive particles are arranged.
6. The method for manufacturing a connection structure according to claim 5, wherein: The first composition is arranged using a pad printing method, and the conductive particles are arranged.
7. The method for manufacturing a connection structure according to claim 6, wherein: The pad printing method uses a flat plate gravure.
8. The method for manufacturing a connection structure according to claim 7, wherein: The step of preparing the first composition and preparing the conductive particles comprises: The first composition is disposed on the upper surface and the concave portion of the flat plate gravure, and the conductive particles are disposed in the concave portion of the flat plate gravure; transferring the first composition and the conductive particles to a pad; and The conductive particles are arranged so as to contact the first electrode or the second electrode.
9. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The viscosity of the first composition is higher than the viscosity of the second composition.
10. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The step of disposing the first composition and the conductive particles includes mixing the conductive particles in the first composition in an amount ranging from 20 volume % to 60 volume %.
11. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition includes a free radical polymerizable resin.
12. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The second composition includes an ene / thiol curable resin containing an ethylenically unsaturated compound and a thiol compound, wherein a curing component of at least one of the ethylenically unsaturated compound and the thiol compound is a 9,9-diarylfluorene compound.
13. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition and the second composition contain a photocuring initiating component.
14. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The step of curing the first composition and the second composition includes irradiating light.
15. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition and the second composition contain a shielding portion curable active compound.
16. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The first composition contains an anaerobic curing initiating component.
17. The method for producing a connection structure according to any one of claims 1 to 4, wherein: The step of curing the first composition and the second composition is performed simultaneously with the pressing.
18. The method for producing a connection structure according to any one of claims 1 to 4, wherein: In the pressing step, the conductive particles are in contact with the first electrode and the second electrode.