Self-adhesive surface protection film
By using an adhesive layer of polypropylene-based resin and block copolymer in the adhesive film, the problem of balance between adhesive force and dischargeability is solved, and effective protection of the uneven surface covering and processability are achieved.
Patent Information
- Application Number
- CN201910491827.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2012-04-10
- Filing Date
- 2013-04-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
After improving the adhesive force, the existing adhesive film is prone to local elongation or deformation in the rolled state, and it is difficult to meet the protection needs of uneven surface coverings such as prisms.
Polypropylene resin is used as the base material layer, and styrene elastomer and polyethylene resin are combined as the adhesive layer. By adjusting the resin type and mixing ratio, a mixture of 35% to 99% styrene elastomer and 1% is formed. ~65% polyethylene resin block copolymer ensures the adhesion and deliverability of the adhesive layer.
It achieves strong adhesion to various covering bodies, avoids elongation or deformation of the film in the rolled state, improves processing suitability, and is suitable for protecting items with uneven surfaces such as prism sheets.
Smart Images

Figure BDA0002087290040000191 
Figure BDA0002087290040000201 
Figure HDA0002087290050000011
Abstract
Description
[0001] The present application is a divisional application of an application filed on April 2, 2013, with application number 201380019463.6 and invention name “Self-adhesive surface protection film”. Technical Field
[0002] The present invention relates to an adhesive film. The adhesive film of the present invention is suitable for the following situations: protecting components such as prism sheets used in optical applications, synthetic resin plates (e.g., for building materials), stainless steel plates (e.g., for building materials), aluminum plates, film-coated plywood, steel plates, glass plates, home appliances, precision machinery, and the surface of automobile bodies during manufacturing, for protecting articles from scratches during stacking, storage, transportation, and conveying in the manufacturing process, and for protecting articles from scratches during secondary processing (e.g., bending processing, pressing processing). Background Art
[0003] Adhesive films for the purpose of protecting the surface of a covering have been used in the processing, storage, and transportation of building materials, electrical and electronic products, and automobiles. Such adhesive films must have good adhesion and be easily peeled off after use without contaminating the surfaces with the adhesive.
[0004] The above-mentioned covering bodies have gradually diversified in recent years, and not only objects with smooth covering surfaces but also objects with uneven surfaces are common. Examples of covering bodies with uneven surfaces include prism-shaped lens parts of prism sheets used in optical components. For covering bodies with uneven surfaces such as prism sheets, in order to exhibit sufficient adhesive force for use, it can be considered to increase the adhesive force of the adhesive layer so that adhesive force can be obtained even if the contact area is small.
[0005] In order to improve the adhesion of the adhesive layer, a styrene-based elastomer having high adhesion can be used as a main component as a resin. However, if the adhesion of the adhesive layer is improved, problems such as sticking, local elongation, or deformation of the film may occur when the film is stored in a roll state and then delivered.
[0006] As the above-mentioned countermeasures, studies have been conducted on adding fluorine-based resins, silicone-based resins (for example, refer to Patent Document 1, etc.), ultrahigh molecular weight polydimethylsiloxane (for example, refer to Patent Document 2, etc.), saturated fatty acid bisamide (for example, refer to Patent Document 3, etc.), etc. to the base material layer. However, these resins are likely to migrate into the adhesive layer when stored in a rolled state, and concerns about reduced adhesion or contamination of the covering body cannot be eliminated.
[0007] In addition, studies have also been conducted on adding polyethylene resins to the adhesive layer (for example, refer to Patent Document 4, Patent Document 5, etc.), but none of them can meet the above-mentioned problems of satisfactory adhesion to the prism and storing the film in a roll state and then delivering the film.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2008-81589
[0011] Patent Document 2: Japanese Patent Application Publication No. 2008-308559
[0012] Patent Document 3: Japanese Patent No. 4565058
[0013] Patent Document 4: Japanese Patent Application Laid-Open No. 08-73822
[0014] Patent Document 5: Japanese Patent Application Publication No. 2007-161882 Summary of the invention
[0015] Problem that the invention aims to solve
[0016] The problem to be solved by the present invention is to provide a self-adhesive surface protection film which exhibits strong adhesion to a covering body, can be used for various covering bodies, and is not prone to problems such as local elongation or deformation of the film when the adhesive film is stored in a roll state and then delivered, and has excellent processing suitability of the film.
[0017] Solutions for solving problems
[0018] As a result of intensive studies, the present inventors have found that the above-mentioned problems can be solved by setting the type and compounding ratio of the resin used in the adhesive layer to a predetermined range, thereby arriving at the present invention.
[0019] That is, the present invention relates to a self-adhesive surface protection film, characterized in that it is formed by laminating an adhesive layer on one side of a substrate layer formed of a polypropylene resin and laminating a release layer on the opposite side by coextrusion, the resin constituting the above-mentioned adhesive layer contains at least a styrene-based elastomer and a polyethylene-based resin, the above-mentioned styrene-based elastomer is a hydrogenated product of a block copolymer having a styrene-based polymer block and a butadiene-based polymer block, or a hydrogenated product of a block copolymer having a styrene-based polymer block and a random copolymer block of styrene and butadiene, the above-mentioned polyethylene-based resin is an ethylene homopolymer and / or an ethylene-α-olefin copolymer, the content of the styrene-based elastomer in the above-mentioned adhesive layer is 35% by mass or more and 99% by mass or less, the content of the polyethylene-based resin is 1% by mass or more and 65% by mass or less, and the sum of the ethylene component in the styrene-based elastomer and the polyethylene-based resin in the adhesive layer components is 35% by mass or more and less than 70% by mass.
[0020] According to the present invention, a self-adhesive surface protection film can be obtained which exhibits strong adhesion to a covering body and can be used for various covering bodies. Moreover, when the adhesive film is stored in a roll state and then the film is fed out, problems such as local elongation or deformation of the film are not easily generated, and the film has excellent processing suitability.
[0021] In this case, the flexural modulus of the ethylene-based resin used in the adhesive layer is preferably 10 MPa or more and less than 90 MPa.
[0022] In this case, the MFR (190° C., 2.16 kgf) of the polyethylene resin in the adhesive layer is preferably 0.5 to 8 g / 10 minutes.
[0023] In this case, the MFR (230° C., 2.16 kgf) of the styrene-based elastomer in the adhesive layer is preferably 0.5 to 8 g / 10 minutes.
[0024] In this case, the MFR (230° C., 2.16 kgf) of the polypropylene resin in the base layer is preferably 1.0 to 15 g / 10 min.
[0025] Effects of the Invention
[0026] The adhesive film of the present invention has the following advantages: it has strong adhesion to the covering body and can be used for various covering bodies. Moreover, when the adhesive film is stored in a roll state and then the film is fed out, it is not easy to cause problems such as local elongation or deformation of the film, and the film has excellent processing suitability. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the test sample. DETAILED DESCRIPTION
[0028] Hereinafter, embodiments of the adhesive film of the present invention will be described.
[0029] (Base material layer)
[0030] The adhesive film of the present invention requires a substrate layer having a polypropylene resin as a main component. Examples of the polypropylene resin used herein include crystalline polypropylene, random copolymers or block copolymers of propylene and a small amount of α-olefins, etc. More specifically, examples of the crystalline polypropylene resin include n-heptane-insoluble isotactic propylene homopolymers or copolymers of propylene and other α-olefins containing 60% by mass or more of propylene used in conventional extrusion molding, etc. The propylene homopolymers or copolymers of propylene and other α-olefins can be used alone or in combination.
[0031] The substrate layer preferably contains 60% or more propylene units, more preferably 70% or more, more preferably 80% or more, and particularly preferably 90% or more. When the propylene unit content is less than 60% by mass, the film loses its stiffness and sometimes becomes difficult to handle. In addition, when the propylene unit content is less than 60% by mass or a polyethylene resin is used, the film becomes soft and easily elongated, and problems such as local elongation or deformation of the film are not likely to occur when the film is fed out.
[0032] Here, n-heptane insolubility refers to the crystallinity of polypropylene as an index and also indicates safety. In the present invention, it is a preferred embodiment to use a substance that meets the n-heptane insolubility based on the Ministry of Health, Labor and Welfare Notice No. 20 of February 1978 (the eluted component when extracted at 25°C and 60 minutes is 150 ppm or less [30 ppm or less for substances used at a temperature exceeding 100°C]).
[0033] As the α-olefin copolymer component constituting the copolymer of propylene and other α-olefins, α-olefins having a carbon number of 2 to 8, for example, ethylene or 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene and other C4 or higher α-olefins can be cited. Here, the copolymer is preferably a random copolymer or a block copolymer obtained by polymerizing propylene with one or more of the above α-olefins.
[0034] Furthermore, copolymers of propylene and other α-olefins may be used alone or in combination of two or more.
[0035] The melt flow rate (MFR: 230° C., 2.16 kgf) of the polypropylene resin used is preferably in the range of 1.0 to 15 g / 10 min, more preferably in the range of 2.0 to 10.0 g / 10 min.
[0036] Furthermore, the film scraps generated when the film obtained in the present invention is processed into products can be re-granulated as recycled raw materials and added to the base material layer. By using recycled raw materials, production costs can be reduced.
[0037] (Adhesive layer)
[0038] Adhesive layer of the present invention needs to comprise styrene elastomer in order to show high adhesive force. In addition, in order to show adhesive force and the delivery property of film self-winding state, adhesive layer needs to comprise polyethylene resin. By adding polyethylene resin, the peeling force of the self-adhesive surface side to the demoulding surface can be reduced. In addition, in adhesive layer, in order to control adhesive force, tackifying resin, softener, polystyrene etc. except polyethylene resin can also be mixed as required.
[0039] Regarding the amount of styrene elastomer in the adhesive layer, in order to show the performance of high adhesive force and the delivery property of the film in a self-rolled state, it is necessary to be 35% by mass or more and 99% by mass or less relative to 100% by mass of the adhesive layer component. When it is lower than 35% by mass, the adhesive force decreases and it is difficult to obtain the required adhesive force. The amount of styrene elastomer in the adhesive layer is preferably in the range of 38% by mass or more and 95% by mass or less. More preferably, it is in the range of 40% by mass or more and 90% by mass or less.
[0040] Examples of styrene-based elastomers include hydrogenated products of ABA-type block polymers such as styrene-butadiene-styrene copolymers, hydrogenated products of AB-type block polymers such as styrene-butadiene copolymers, hydrogenated products of styrene-based random copolymers such as styrene-butadiene rubber, etc. It should be noted that these hydrogenated products may be partial hydrogenated products or complete hydrogenated products.
[0041] The styrene content in the styrene elastomer is preferably 5% by mass or more and 40% by mass or less. When it is less than 5% by mass, granulation becomes difficult when preparing the resin, and when it exceeds 40% by mass, the adhesive force decreases, and it sometimes becomes difficult to obtain the desired adhesive force. It should be noted that the styrene content in the styrene elastomer is preferably in the range of 8% by mass or more and 35% by mass or less, and more preferably in the range of 10% by mass or more and 30% by mass or less.
[0042] On the other hand, it is ideal that the ethylene content in the styrene elastomer is 15% by mass or more and 70% by mass or less. The ethylene content in the styrene elastomer has the effect of improving the compatibility with the polyethylene resin and the effect of improving the delivery of the film in the self-rolled state. Therefore, it can be considered that when the amount of the ethylene content is large, the effect of improving the delivery property tends to become larger. In addition, it can be considered that the ethylene content in the styrene elastomer also greatly contributes to the expression of the adhesive force. When the amount of the ethylene content exceeds 70% by mass, there is a concern that the adhesive force of the adhesive layer becomes too high.
[0043] In addition, it is preferred that a butene component is present in the styrene-based elastomer. When the butene component is 50% by mass or more, the adhesive force tends to be less likely to decrease when the polyethylene-based resin is added, which is preferred.
[0044] The melt flow rate (MFR: 230° C., 2.16 kgf) of the styrene-based elastomer used is preferably in the range of 0.5 to 8 g / 10 minutes, more preferably in the range of 2.0 to 7.0 g / 10 minutes, in terms of film forming properties.
[0045] The amount of the polyethylene resin in the adhesive layer needs to be 1% by mass or more and 65% by mass or less in order to show high adhesive force and the delivery property of the film in a self-rolled state. When the amount of the polyethylene resin in the adhesive layer exceeds 65% by mass, the adhesive force decreases and it becomes difficult to obtain the desired adhesive force. The amount of the polyethylene resin in the adhesive layer is preferably in the range of 3% by mass or more and 60% by mass or less.
[0046] As polyethylene resins, low-density polyethylene, copolymers of ethylene and α-olefins, etc. can be cited. Among them, low-density polyethylene, especially linear low-density polyethylene called LLDPE, and ultra-low-density polyethylene called VLDPE can maintain adhesion and improve the delivery of the film, so they are preferred. They are introduced into the ethylene chain by copolymerizing α-olefins, and according to the type and copolymerization amount of α-olefins, softness can be given to polyethylene resins.
[0047] Examples of the α-olefin include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene.
[0048] In the adhesive layer of the present invention, the sum of the ethylene component and the polyethylene resin in the styrene elastomer is 35% by mass or more and less than 70% by mass in the adhesive layer composition. When the sum of the ethylene component and the polyethylene resin is 70% by mass or more in the adhesive layer composition, the adhesive force is reduced and sufficient adhesive force cannot be obtained. When the sum of the ethylene component and the polyethylene resin is less than 35% by mass in the adhesive layer composition, the peeling force of the film adhesive layer to the release layer becomes high. Preferably, the sum of the ethylene component and the polyethylene resin is 40% by mass or more and less than 70% by mass in the adhesive layer composition. More preferably, the sum of the ethylene component and the polyethylene resin is 45% by mass or more and less than 65% by mass in the adhesive layer composition. Particularly preferably, the sum of the ethylene component and the polyethylene resin is 45% by mass or more and less than 63% by mass in the adhesive layer composition.
[0049] The bending modulus of the polyethylene resin is preferably 10 MPa or more and less than 90 MPa. When it is less than 10 MPa, the delivery property of the film in the self-wound state is reduced, and when it is 90 MPa or more, the adhesive layer becomes hard and there is a tendency for the adhesive force to decrease. The bending modulus of the polyethylene resin is preferably in the range of 15 MPa to 80 MPa, and more preferably in the range of 20 MPa to 70 MPa.
[0050] In order to set the bending modulus to the above range, adjusting the ethylene component in the polyethylene resin is a strategy. From the above viewpoint, the ethylene component in the polyethylene resin is preferably 70% by mass or more. The ethylene component of the polyethylene resin is more preferably 75% by mass or more, and further preferably 80% by mass or more. In addition, the ethylene content of the polyethylene resin is preferably 98% by mass or less, more preferably 96% by mass or less, further preferably 95% by mass or less, and particularly preferably 94% by mass or less. When the ethylene component in the polyethylene resin is less than 70% by mass, there is a tendency that the improvement effect of the delivery of the film in the self-winding state becomes smaller. As an example of a polyethylene resin with an ethylene component of 70% by mass or more in the polyethylene resin, CX3007, VL100, etc. manufactured by Sumitomo Chemical Co., Ltd. can be cited.
[0051] The density of the polyethylene resin is preferably 850 kg / m 3 ~920kg / m 3 , more preferably 860kg / m 3 ~910kg / m 3 , particularly preferably 870kg / m 3 ~908kg / m 3 , the most preferred is 880kg / m 3 ~906kg / m 3 By setting it as the said range, it becomes easy to achieve both good adhesiveness and delivery property.
[0052] The melt flow rate (MFR: 190°C, 2.16 kgf) of the polyethylene resin used is preferably in the range of 0.5 to 8 g / 10 min, more preferably in the range of 0.8 to 7.0 g / 10 min. By setting it in the above range, film formation with uniform thickness of each layer becomes easy.
[0053] The adhesive layer may also contain polyolefin resins other than polyethylene resins, and the types thereof are not particularly limited, and examples thereof include crystalline polypropylene, copolymers of propylene and a small amount of α-olefins, etc. These resins generally have a tendency to reduce adhesive force even when mixed in small amounts, and are therefore preferably mixed in a ratio of 1% by mass to 20% by mass.
[0054] As the tackifying resin, for example, aliphatic hydrocarbon resins, aromatic hydrocarbon resins, terpene resins, coumarone-indene resins, styrene resins, rosin resins, etc. can be cited. The molecular weight of the tackifying resin can be appropriately set without particular restrictions. When the molecular weight becomes small, there is a concern that the material migration from the adhesive layer to the cover, heavy peeling, etc. will occur. On the other hand, when the molecular weight becomes large, there is a tendency to lack the effect of improving the adhesive force. Therefore, the number average molecular weight of the tackifying resin is preferably about 1000 to 100,000. The number average molecular weight can be measured by gel permeation chromatography (standard substance: polystyrene) or the like.
[0055] About the compounding amount of the tackifier resin in the adhesive layer, relative to 100% by mass adhesive layer components, preferably the scope of more than 5% by mass and less than 20% by mass. When the compounding amount of the tackifier resin is made to exceed 20% by mass, the tackifier resin is due to low molecular weight, so the melt viscosity is extremely reduced, and the lamination of the substrate layer with polypropylene resin as the main component becomes difficult when the coextrusion film making using T molds etc. is carried out, and the adhesive layer is sticky, and the delivery of the film in the self-winding state has a tendency to be difficult to improve. In addition, when the compounding amount of the tackifier resin in the adhesive layer is less than 5% by mass, even if compounding is also difficult to contribute to the adhesive force change of the adhesive layer. Therefore, the compounding amount of the tackifier resin is preferably more than 6% by mass and less than 20% by mass. More preferably, the scope of more than 6% by mass and less than 15% by mass.
[0056] When the melt viscosity tends to decrease due to the addition of a tackifier resin to the adhesive layer, the difference in melt viscosity between the substrate layer and the adhesive layer can be improved by adding about 1% to 15% by mass of a polystyrene resin to the adhesive layer, making it easier to laminate. The polystyrene resin compounding amount is preferably 3% to 12% by mass, more preferably 5% to 10% by mass.
[0057] As a softener, for example, low molecular weight diene polymers, polyisobutylene, hydrogenated polyisoprene, hydrogenated polybutadiene, their derivatives, polybutene, etc. can be listed. The molecular weight of the softener can be appropriately set without particular restrictions. When the molecular weight becomes small, there is a concern that the material migration from the adhesive layer to the cover, heavy peeling, etc. may occur. On the other hand, when the molecular weight becomes large, there is a tendency to lack the effect of improving the adhesive force. Therefore, the number average molecular weight of the softener is preferably about 1000 to 100,000. The number average molecular weight can be measured by the same method as the case of the tackifying resin.
[0058] In addition, the tackifying resin and softening agent used in the adhesive layer may be liquid or powder depending on the type, and may sometimes contaminate the extruder during extrusion. This problem can be improved by using the tackifying resin and softening agent in a master batch with a polyethylene resin or a polyolefin resin. Therefore, the tackifying resin and softening agent are preferably used in a master batch with a polyethylene resin or a polyolefin resin.
[0059] The adhesive force of the adhesive film (adhesive layer) of the present invention is preferably in the range of 200 cN / 25mm to 1000 cN / 25mm for acrylic plates at 23°C, which is preferably used for various covers. When the adhesive force is less than 200 cN / 25mm, curling occurs when the cover is used for protection, and the function as a protective film cannot be fulfilled. On the other hand, when the adhesive force exceeds 1000 cN / 25mm, when the film is peeled off from the cover, there is a concern that it cannot be peeled off smoothly.
[0060] In addition, at 23°C, the range of 2cN / 25mm to 20cN / 25mm for the prism sheet is preferred in consideration of use. When the adhesive force is less than 2cN / 25mm, curling occurs during protection, and the function as a protective film cannot be fulfilled. On the other hand, when the adhesive force exceeds 20cN / 25mm, there is a concern that the film cannot be peeled off smoothly when peeling. The adhesive force can be appropriately set by changing the resin composition, thickness, etc. of the adhesive layer.
[0061] The adhesive layer of the present invention may also contain known additives as required. For example, it may contain lubricants, anti-blocking agents, heat stabilizers, antioxidants, antistatic agents, light stabilizers, impact resistance modifiers, etc. However, these components have low molecular weights and sometimes ooze out on the surface of the adhesive layer to reduce the adhesive force of the adhesive layer. Therefore, when using additives, it is preferred to make the amount of low molecular weight substances on the surface of the adhesive layer less than 1 mg / m 2 .
[0062] The determination of low molecular weight substances on the adhesive layer surface is carried out according to the following steps. After washing the adhesive layer surface with an organic solvent such as ethanol that does not corrode the resin constituting the adhesive layer, the organic solvent is removed from the washing liquid by an evaporator, etc., and the value obtained by weighing the residue is divided by the surface area of the adhesive layer surface after washing to obtain the low molecular weight substances on the adhesive layer surface. The residue exists at 1 mg / m 2 When the above conditions are met, foreign matter will be present between the surface of the adhesive layer and the surface of the covering body, which will reduce the contact area with the covering body and reduce the van der Waals force, thus reducing the adhesive force, which is not preferred. When adding additives, it is necessary to select additives such as polymers, or study the amount and method of addition, so that the transfer and transfer of low molecular weight substances (foreign matter) to the adhesive layer will not occur.
[0063] (Release layer)
[0064] The adhesive film of the present invention has a release layer on the opposite side of the adhesive layer stacked on one side of the substrate layer. Thus, even if the adhesive films are overlapped with each other, the adhesion of the adhesive films to each other can be suppressed. By arranging the release layer, it is particularly difficult to produce problems such as local elongation or deformation of the film when the adhesive film is stored in a roll state and then the film is sent out, and a film with excellent processing suitability can be made. In order to prevent the adhesion of the adhesive films to each other even if the adhesive films are overlapped with each other, it is effective to form a surface concavo-convex on the release layer to reduce the contact area with the adhesive layer.
[0065] The mold release layer preferably contains a polypropylene resin as a main component (about 50% by mass or more). Specific examples of the polypropylene resin include propylene-ethylene block copolymers.
[0066] In order to form the above-mentioned surface concavoconvex on the release layer, it is effective to mix incompatible resins in the polypropylene resin. Thus, a layer with rough surface can be formed in a matte shape. It should be noted that, as the polypropylene resin, when using propylene-ethylene block copolymer, the same effect can be expected without using incompatible resins in the polypropylene resin. It should be noted that, of course, in the propylene-ethylene block copolymer, a resin incompatible with the polypropylene resin can also be further added.
[0067] As the resin incompatible with polypropylene resin, α-olefin (co)polymers with carbon number of more than 4 such as low-density polyethylene, 4-methyl-1-pentene (co)polymers can be suitably used. In addition, copolymers of linear low-density polyethylene, high-density polyethylene, ethylene and a small amount of α-olefin, copolymers of ethylene and vinyl acetate, polystyrene, polyester resins, polyamide resins, etc. can be listed. Especially when using 4-methyl-1-pentene (co)polymers, not only the surface of the release layer is made rough with matte shape, but also the surface free energy of the film surface is reduced, thereby further improvement of strippability can be expected.
[0068] Taking into account the resin composition of the adhesive layer of the present invention, it is preferred that the three-dimensional average surface roughness SRa of the surface of the release layer be set to 0.10 μm or more and 0.50 μm or less. Thus, the blocking resistance and the protective performance of the cover can be improved. When the surface roughness of the release layer is less than 0.10 μm, the delivery of the film when the film is made into a roll form sometimes deteriorates. When the surface roughness of the release layer is higher than 0.50 μm, the surface concavo-convex of the release layer is transferred to the surface of the adhesive layer, and sometimes the adhesive force is significantly reduced. At this time, it is more preferred to form a surface with a surface average surface roughness SRa of 0.25 μm or more and 0.45 μm or less.
[0069] The three-dimensional average surface roughness SRa of the release layer surface refers to the average roughness of the center plane when the surface roughness curve is approximated by a sine curve, and can be measured by a surface roughness measuring device or the like.
[0070] (Self-adhesive surface protection film)
[0071] The self-adhesive surface protection film of the present invention is composed of a substrate layer, an adhesive layer, and a release layer containing the above-mentioned resin component. The thickness of the self-adhesive surface protection film of the present invention is preferably 10 μm or more and 150 μm or less, more preferably 15 μm or more and 120 μm or less, and further preferably 20 μm or more and 100 μm or less. When the total thickness of the film is too thin, it may deteriorate during handling, and when it is too thick, it may form a film with high rigidity, deteriorated handling properties, and disadvantageous cost.
[0072] The thickness of the substrate layer of the present invention is preferably 5 μm or more and less than 100 μm, more preferably 10 μm or more and 75 μm or less, and further preferably 15 μm or more and 55 μm or less. When the thickness of the substrate layer is less than 5 μm, the stiffness becomes weak, and wrinkles are easily generated when the protective film is attached to the cover body, and there is a problem that sufficient adhesive strength cannot be obtained. When the thickness is more than 100 μm, a film disadvantageous in terms of cost is formed.
[0073] The thickness of the adhesive layer of the present invention is preferably 1 μm or more and less than 30 μm. When the thickness of the adhesive layer is less than 1 μm, stable film formation based on coextrusion becomes difficult, and when it is more than 30 μm, a film that is disadvantageous in terms of cost is formed. At this time, when increasing the adhesive force, it is preferred to increase the thickness of the adhesive layer in consideration of its viscosity. By increasing the thickness of the adhesive layer, the contact area with the covering body tends to become larger. The thickness of the adhesive layer is preferably 2 μm or more and 20 μm or less, more preferably 3 μm or more and 15 μm or less, and particularly preferably 4 μm or more and 8 μm or less.
[0074] The thickness of the release layer of the present invention is preferably 1 μm or more and less than 30 μm. When the thickness of the release layer is less than 1 μm, stable film formation by coextrusion becomes difficult, and when it is 30 μm or more, a thin film that is disadvantageous in terms of cost is formed. The thickness of the release layer is preferably 2 μm or more and 20 μm or less, and more preferably 3 μm or more and 15 μm or less.
[0075] When the peeling force of the adhesive surface of the adhesive film of the present application to the demolding surface is in the range of 250 cN / 40 mm or less at 23°C, it is preferred from the viewpoint of the delivery of the film when the adhesive film is made into a roll form. When the peeling force exceeds 250 cN / 40 mm, when the film is delivered when the adhesive film is made into a roll form, problems such as local elongation or deformation of the film occur. It is more preferably 200 cN / 40 mm or less. It should be noted that the lower limit of the peeling force of the adhesive surface of the adhesive film to the demolding surface is, as a realistic value, about 1 cN / 40 mm, and further about 5 cN / 40 mm.
[0076] The self-adhesive surface protection film of the present invention is composed of each layer of a substrate layer, an adhesive layer, and a release layer containing the above-mentioned resin components. The resin constituting each layer can be obtained, for example, as follows: using a single-screw or twin-screw extruder, etc., directly feeding it to a feed block type or a multi-manifold type T-die in a molten state, and extruding it in layers of three or more layers (substrate layer, adhesive layer, release layer), thereby obtaining it. Regarding the temperature of the extruder of each layer, in order to make each layer in a molten state, it can be appropriately adjusted by appropriately considering the molding temperature of the components used in each layer, for example, it can also be adjusted in the range of 200°C to 260°C. The temperature of the T-die can be the same as the above-mentioned temperature. The speed of collecting from the T-die to the casting roll can be any speed that makes each layer a suitable thickness, for example, 10m / min to 200m / min, preferably 10m / min to 100m / min.
[0077] The adhesive film of the present invention is suitable for handling in the form of a roll. There is no particular restriction on the upper limit of the width and length of the film roll. From the perspective of ease of handling, it is generally preferred that the width is 1.5 m or less and the roll length is 5000 m or less when the film thickness is 40 μm. In addition, as a winding core, a plastic core or a metal core of 3 inches, 6 inches, 8 inches, etc. can usually be used. In addition, from the perspective of processing suitability, a film roll with a length of more than 200 m and a width of more than 450 mm is preferably wound.
[0078] The adhesive film of the present invention can be used in the following situations: protecting components such as prism sheets used in optical applications, synthetic resin plates (e.g., for building materials), stainless steel plates (e.g., for building materials), aluminum plates, film-coated plywood, steel plates, glass plates, home appliances, precision machinery, and the surface of automobile bodies during manufacturing; protecting items from scratches when they are stacked, stored, or transported, or conveyed in the manufacturing process; and protecting items from scratches during secondary processing (e.g., bending, pressing).
[0079] This application claims the priority right based on Japanese Patent Application No. 2012-89184 filed on April 10, 2012. The entire contents of the specification of Japanese Patent Application No. 2012-89184 filed on April 10, 2012 are incorporated herein by reference.
[0080] Example
[0081] The present invention is further described below with reference to examples. However, the present invention is not limited to the following examples unless it exceeds the gist of the present invention. It should be noted that the evaluation methods of the physical properties in the following examples and comparative examples are as follows.
[0082] (1) Evaluation of Adhesion
[0083] The pressure-sensitive adhesive tape and pressure-sensitive adhesive sheet test method was measured by the following method according to JIS-Z-0237 (2000).
[0084] As the covering body, an acrylic plate (manufactured by Mitsubishi Rayon Co., Ltd.: Acrylite (registered trademark) 3 mm thick) 50 mm × 150 mm and a prism sheet (the lens portion is composed of a triangular prism, the height of the triangular prism is 25 μm, and the width of the triangular prism is 50 μm) 50 mm × 150 mm were prepared. As a test piece, a test piece with a size of 150 mm in the winding direction during film manufacturing and 25 mm in the direction orthogonal to it was cut out.
[0085] A rubber roller with a mass of 2000g (the roller surface is covered with a rubber layer with a spring hardness of 80Hs and a thickness of 6mm, a width of 45mm, and a diameter (including the rubber layer) of 95mm) is used to press the cover and the test piece together by reciprocating once at a speed of 5mm / second. After pressing, the sample is placed in an environment with a temperature of 23°C and a relative humidity of 65% for 30 minutes, and the "Autograph (registered trademark)" (AGS-J) manufactured by Shimadzu Corporation is used to peel the sample 180 degrees at a speed of 300mm / minute, and the resistance value at this time is used as the adhesion [cN / 25mm]. 180-degree peeling means that the peeling angle between the acrylic plate and the film is kept at 180 degrees when measuring the resistance value during peeling.
[0086] During the measurement, a polyester sheet with a thickness of 190 μm and a size of 25 mm × 170 mm was prepared as a chuck for the measurement sample. The polyester sheet was attached to the end of one side of the test piece of the measurement sample formed by crimping the test piece and the acrylic plate with a transparent tape at a width of 15 mm at the attachment site to form a chuck for the measurement. The schematic diagram of the measurement sample is shown in Figure 1 The measurement was performed on three samples made of each film produced in Examples and Comparative Examples, and the average value thereof was taken as the adhesive strength of the sample. The prism sheet was measured in the same manner.
[0087] (2) Evaluation of peeling force
[0088] A double-sided adhesive tape (manufactured by Nitto Denko Corporation) was affixed to the entire surface of an acrylic plate (manufactured by Mitsubishi Rayon Co., Ltd.: Acrylite (registered trademark) 3 mm thick) measuring 50 mm × 150 mm, and a test piece measuring 150 mm (in the winding direction during film manufacturing) × 50 mm (in a direction perpendicular to the winding direction during film manufacturing) was affixed to the other side of the double-sided adhesive tape so that the adhesive surface of the test piece faced the test piece.
[0089] As a new test piece, a test piece with a length of 150 mm in the winding direction and 40 mm in the direction perpendicular to it during film manufacturing was cut out. After overlapping its adhesive surface with the demoulding surface of the test piece attached to the acrylic plate via the double-sided adhesive tape, a rubber roller with a mass of 2000 g (the roller surface is covered with a rubber layer with a spring hardness of 80 Hs and a thickness of 6 mm, a width of 45 mm, and a diameter (including the rubber layer) of 95 mm) was used to press the demoulding surface and the test piece together by reciprocating once at a speed of 5 mm / second. After pressing, a total area of 4000 mm with a length of 100 mm in the winding direction and 40 mm in the direction perpendicular to it was formed. 2 A load of 60 kg was applied and the sample was placed in an environment of 40°C and 65% relative humidity for 24 hours, then cooled to 23°C. The sample was peeled 180 degrees at a speed of 300 mm / min using "Autograph (registered trademark)" (AGS-J) manufactured by Shimadzu Corporation. The resistance value at this time was taken as the peeling force [cN / 40mm].
[0090] During the measurement, a polyester sheet with a thickness of 190 μm and a size of 40 mm × 170 mm was prepared as a chuck for the measurement sample, and a 15 mm wide adhesive tape was used to stick the end of the 150 mm × 40 mm test piece to the sticking part as the chuck for the measurement. The measurement was carried out 3 times for one sample, and the average value was taken as the peeling force of the sample.
[0091] (3) Self-winding delivery
[0092] After cutting to obtain a 550 mm wide, 500 m roll, store it in a roll state for 7 days in a light-shielded environment at a temperature of 23°C and a humidity of 75%. Just after unwinding the film roll 300 m onto another plastic core (9 cm in diameter), hold the end of the film by hand and pull it to unwind 3 m. Visually check whether there is local elongation or deformation of the film during unwinding. The case of no local elongation or deformation is rated as ○ (good), and the case of local elongation or deformation is rated as × (bad).
[0093] (4) Determination of MFR of resin
[0094] The measurement was conducted in accordance with JIS-K7210.
[0095] (5) Determination of flexural elastic modulus of resin
[0096] The measurement was carried out according to ASTM D747-70.
[0097] (6) Determination of ethylene content in styrene elastomers
[0098] About 330 mg of resin sample was dissolved in deuterated chloroform and measured 13 C-NMR (manufactured by BRUKER, AVANCE500). The amount of ethylene component in the styrene-based elastomer was identified using the obtained measurement results.
[0099] [Example 1]
[0100] (Production of base material layer)
[0101] Homopolypropylene resin (manufactured by Sumitomo Chemical Co., Ltd.: FLX80E4, 230°C MFR: 7.5 g / 10 min) was used as 100% by mass. The single screw extruder was used for melt extrusion at 240°C to prepare the base material layer.
[0102] (Production of Adhesive Layer)
[0103] An adhesive layer was prepared by melt-extruded at 210°C using a 45 mmφ single-screw extruder with 40% by mass of a styrene-based elastomer (a hydrogenated block copolymer of styrene and butadiene, manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12% by mass, ethylene component ratio of 18% by mass, MFR at 230°C: 4.5 g / 10 min), 50% by mass of an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: CX3007, MFR at 190°C: 3.7 g / 10 min, elastic modulus: 26 MPa), and 10% by mass of a petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: Alcon (registered trademark) P125).
[0104] (Production of release layer)
[0105] A release layer was prepared by melt extrusion of 90% by mass of a propylene-ethylene block copolymer (BC3HF manufactured by Japan Polypropylene Corporation) and 10% by mass of a low-density polyethylene resin (R300 manufactured by Ube Industries, Ltd.) at 230°C using a 65 mmφ single-screw extruder.
[0106] (Thin film production)
[0107] The substrate layer, adhesive layer, and release layer were extruded in layers in a 3-layer T-die (feeder type, lip width 850 mm, lip gap 1 mm) at 245°C while being melted by each extruder. The extruded film was taken up at a speed of 20 m / min on a casting roll at a temperature of 30°C, cooled and solidified, and three types of 3-layer unstretched films with a substrate layer thickness of 28 μm, an adhesive layer thickness of 6 μm, a release layer thickness of 6 μm, a film width of 600 mm, and a film length of 1100 m were obtained. The film was then cut at a speed of 50 m / min while applying a contact pressure of 50 N relative to the film width with a rubber roller under a taking-up tension of 40 N, thereby obtaining an unstretched film with a film width of 550 mm and a film length of 500 m.
[0108] [Example 2]
[0109] The substrate layer and the release layer were the same as in Example 1, but the adhesive layer was changed to the following content. By the same production method as in Example 1, three types of three-layered unstretched films were obtained.
[0110] (Production of Adhesive Layer)
[0111] 60% by mass of a styrene-based elastomer (manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12% by mass, ethylene component ratio of 18% by mass, 230°C MFR: 4.5 g / 10 min) and 40% by mass of an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: CX3007, 190°C MFR: 3.7 g / 10 min, elastic modulus: 26 MPa) were melt-extruded at 210°C using a 45 mmφ single-screw extruder to form an adhesive layer.
[0112] [Example 3]
[0113] The substrate layer and the release layer were the same as in Example 1, but the adhesive layer was changed to the following content. By the same production method as in Example 1, three types of three-layered unstretched films were obtained.
[0114] (Production of Adhesive Layer)
[0115] An adhesive layer was prepared by melt-extruded at 210°C using a 40 mmφ single-screw extruder with 40% by mass of a styrene-based elastomer (a hydrogenated block copolymer of styrene and butadiene, manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12% by mass, ethylene component ratio of 18% by mass, MFR at 230°C: 4.5 g / 10 min), 50% by mass of an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: VL100, MFR at 190°C: 0.8 g / 10 min, elastic modulus: 64 MPa), and 10% by mass of a petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: Alcon (registered trademark) P125).
[0116] [Example 4]
[0117] The substrate layer and the release layer were the same as in Example 1, but the adhesive layer was changed to the following content. By the same production method as in Example 1, three types of three-layered unstretched films were obtained.
[0118] (Production of Adhesive Layer)
[0119] An adhesive layer was prepared by melt-extruded at 210°C a styrene elastomer (TUFTEC (registered trademark) H1041 manufactured by Asahi Kasei Chemicals Corporation, 30% styrene component ratio, 49% ethylene component ratio, 230°C MFR: 5.0 g / 10 min), 85% by mass, an ethylene-α-olefin copolymer (CX3007 manufactured by Sumitomo Chemical Co., Ltd., 0.8 g / 10 min at 190°C, elastic modulus: 26 MPa), and 10% by mass of a petroleum resin (Alcon (registered trademark) P125 manufactured by Arakawa Chemical Industries, Ltd.) using a 40 mmφ single-screw extruder.
[0120] [Example 5]
[0121] The base material layer and the release layer remain the same as in Example 1, and the adhesive layer is changed to the following content: the base material layer thickness is set to 26 μm, the adhesive layer thickness is set to 8 μm, and the release layer thickness is set to 6 μm. In addition, three types of three-layer unstretched films are obtained by the same preparation method as in Example 1.
[0122] (Production of Adhesive Layer)
[0123] 60% by mass of a styrene-based elastomer (manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12% by mass, ethylene component ratio of 18% by mass, 230°C MFR: 4.5 g / 10 min) and 40% by mass of an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: CX3007, 190°C MFR: 3.7 g / 10 min, elastic modulus: 26 MPa) were melt-extruded at 210°C using a 45 mmφ single-screw extruder to form an adhesive layer.
[0124] [Example 6]
[0125] The substrate layer and the release layer remain the same as in Example 1, and the adhesive layer is changed to the following content: the thickness of the substrate layer is set to 30μm, the thickness of the adhesive layer is set to 4μm, and the thickness of the release layer is set to 6μm. In addition, three types of three-layer unstretched films are obtained by the same preparation method as in Example 1.
[0126] (Production of Adhesive Layer)
[0127] A styrene-based elastomer (manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12 mass%, ethylene component ratio of 18 mass%, 230°C MFR: 4.5 g / 10 min) 40 mass%, an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: CX3007, 190°C MFR: 3.7 g / 10 min, elastic modulus: 26 MPa) 55 mass% and a petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: Alcon (registered trademark) P125) 5 mass% were melt-extruded at 210°C using a 45 mmφ single-screw extruder to form an adhesive layer.
[0128] [Comparative Example 1]
[0129] The substrate layer and the release layer were the same as in Example 1, but the adhesive layer was changed to the following content. By the same production method as in Example 1, three types of three-layered unstretched films were obtained.
[0130] (Production of Adhesive Layer)
[0131] A styrene-based elastomer (manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12 mass%, ethylene component ratio of 18 mass%, 230°C MFR: 4.5 g / 10 min) 70 mass%, an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: CX3007, 190°C MFR: 3.7 g / 10 min, elastic modulus: 26 MPa) 20 mass% and a petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: Alcon (registered trademark) P125) 10 mass% were melt-extruded at 210°C using a 40 mmφ single-screw extruder to form an adhesive layer.
[0132] [Comparative Example 2]
[0133] The substrate layer and the release layer were the same as in Example 1, but the adhesive layer was changed to the following content. By the same production method as in Example 1, three types of three-layered unstretched films were obtained.
[0134] (Production of Adhesive Layer)
[0135] A styrene-based elastomer (manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12 mass%, ethylene component ratio of 18 mass%, 230°C MFR: 4.5 g / 10 min) 70 mass%, an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: VL100, 190°C MFR: 0.8 g / 10 min, elastic modulus: 64 MPa) 20 mass% and a petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: Alcon (registered trademark) P125) 10 mass% were melt-extruded at 210°C using a 40 mmφ single-screw extruder to form an adhesive layer.
[0136] [Comparative Example 3]
[0137] A styrene-based elastomer (manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12 mass%, ethylene component ratio of 18 mass%, 230°C MFR: 4.5 g / 10 min), 20 mass% of an ethylene-α-olefin copolymer (manufactured by Sumitomo Chemical Co., Ltd.: CX3007, 190°C MFR: 3.7 g / 10 min, elastic modulus: 26 MPa) and 10 mass% of a petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: Alcon (registered trademark) P125) were melt-extruded at 210°C using a 40 mmφ single-screw extruder to form an adhesive layer.
[0138] [Comparative Example 4]
[0139] The substrate layer and the release layer were the same as in Example 1, but the adhesive layer was changed to the following content. By the same production method as in Example 1, three types of three-layered unstretched films were obtained.
[0140] (Production of Adhesive Layer)
[0141] A styrene-based elastomer (manufactured by Asahi Kasei Chemicals Corporation: TUFTEC (registered trademark) H1221, styrene component ratio of 12 mass%, ethylene component ratio of 18 mass%, 230°C MFR: 4.5 g / 10 min) 40 mass%, homopolypropylene (manufactured by Sumitomo Chemical Co., Ltd.: FLX80E4, 190°C MFR: 7.5 g / 10 min) 50 mass% and a petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: Alcon (registered trademark) P125) 10 mass% were melt-extruded at 210°C using a 40 mmφ single-screw extruder to form an adhesive layer.
[0142] The above results are shown in Tables 1 and 2.
[0143] [Table 1]
[0144]
[0145] [Table 2]
[0146]
[0147] As shown in Table 2, the films obtained in Examples 1 to 6 had sufficient adhesive strength for practical use when used as a protective film, and also had good releasability when the film was rolled out.
[0148] On the other hand, the films obtained in Comparative Examples 1 and 2 were not necessarily good in peelability when the films were rolled out. The films obtained in Comparative Examples 3 and 4 were not sufficiently adhesive to the covering. Thus, the films obtained in the comparative examples were all of poor quality and had low practicality.
Claims
1. A self-adhesive surface protection film, characterized in that: The adhesive layer is laminated on one side of a substrate layer formed of a polypropylene resin and a release layer is laminated on the opposite side by coextrusion. The release layer is composed of a polypropylene resin and one or more selected from low-density polyethylene and an α-olefin polymer with a carbon number of 4 or more. The resin constituting the adhesive layer contains at least a styrene-based elastomer and a polyethylene-based resin. The styrene-based elastomer is a hydrogenated block copolymer having a styrene-based polymer block and a butadiene-based polymer block. The polyethylene resin is an ethylene homopolymer and / or an ethylene-α-olefin copolymer. The content of the styrene-based elastomer in the adhesive layer is 35% by mass or more and 99% by mass or less, the content of the polyethylene-based resin is 1% by mass or more and 65% by mass or less, and The sum of the ethylene component in the styrene elastomer and the polyethylene resin in the adhesive layer component is 35% by mass or more and less than 50.8% by mass, At 23° C., the adhesive force of the self-adhesive surface protection film to the prism sheet is 2 cN / 25 mm to 6 cN / 25 mm.
2. The self-adhesive surface protection film according to claim 1, wherein The α-olefin polymer having 4 or more carbon atoms is an α-olefin copolymer having 4 or more carbon atoms.
3. The self-adhesive surface protection film according to claim 1, wherein The polyethylene resin used in the adhesive layer has a bending modulus of 10 MPa or more and less than 90 MPa.
4. The self-adhesive surface protection film according to any one of claims 1 to 3, wherein The polyethylene resin in the adhesive layer has an MFR of 0.5 to 8 g / 10 minutes at 190° C. and 2.16 kgf.
5. The self-adhesive surface protection film according to any one of claims 1 to 3, wherein The MFR of the styrene-based elastomer in the adhesive layer at 230° C. and 2.16 kgf is 0.5 to 8 g / 10 minutes.