A control method for converter double slag smelting
By retaining slag and adding auxiliary materials, the alkalinity and magnesium oxide content of the slag are controlled, combined with low oxygen supply and high-pressure nitrogen blowing, the problem of insufficient splashing and slag release in the converter double slag smelting is solved, and the smelting stability is achieved Improved dephosphorization efficiency.
Patent Information
- Application Number
- CN201810256702.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-03-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2038-03-27
AI Technical Summary
It is difficult to accurately control the early oxygen supply time and slag alkalinity during converter double slag smelting, resulting in insufficient splashing and slag release, affecting the stability of later smelting.
By retaining slag and adding lime or magnesium-containing auxiliary materials, the binary alkalinity and magnesium oxide content of the slag are controlled, the early oxygen supply amount and time are adjusted, and the low oxygen supply intensity and high-pressure nitrogen blown are used to form slag foam to improve slag release quantity.
It effectively avoids early splashing, improves the foaming and slag release of the later slag, and ensures the stability and dephosphorization efficiency of later smelting.
Abstract
Description
Technical Field
[0001] The invention relates to a control method for converter double-slag smelting, which is suitable for controlling early splashing of the converter and smelting of low-phosphorus steel grades. Background Art
[0002] The double-slag smelting technology of converter is an effective control measure for controlling metal splashing in the early stage of converter smelting and removing the slag formed in the early stage for smelting low-phosphorus steel grades. However, the difficulty of double-slag smelting lies in how to accurately control the time of stopping oxygen supply in the early stage, how to control the basicity of the slag in the early stage, and how to adjust the influence of the slag foaming state after lifting the gun on slag discharge. If it is judged based on manual experience, splashing may occur due to late lifting of the gun, or insufficient slag discharge due to premature lifting of the gun, and the slag with high SiO2 content in the early stage cannot be discharged, which in turn affects the stability of the later smelting. Summary of the invention
[0003] The technical problem to be solved by the present invention is to overcome the shortcomings of the above-mentioned technology and provide a control method for converter double slag smelting which can effectively avoid splashing during the early oxygen supply period, improve the slag foaming in the later period and ultimately increase the slag discharge amount.
[0004] In order to solve the above technical problems, the technical solution proposed by the present invention is: a control method for converter double slag smelting, comprising the following steps:
[0005] The first step is to leave part or all of the slag from the previous furnace for the current furnace. According to the silicon content of the molten iron of the current furnace, the binary basicity of the previous slag and the content of magnesium oxide in the previous furnace, lime and / or magnesium-containing auxiliary materials are added as slag-making in the early stage of the current furnace. The amount of slag-making added in the early stage makes the binary basicity R of the slag in the early stage of the current furnace meet 1≤R≤1.3 and the content of magnesium oxide is greater than 6%;
[0006] Among them, the amount of slag left in the upper furnace is: M 留渣量 =R×(M 铁水质量 ×Si 铁水 %×2.14) / (CaO 上炉炉渣 %-R×SiO 2上炉炉渣 %); When calculating the amount of slag to be retained and whether lime and magnesium-containing auxiliary materials need to be added in the early stage, it is necessary to know the content of CaO and SiO2 in the slag of the upper furnace, and the composition of molten iron and slag can be obtained through chemical analysis. The magnesium oxide content in the early slag can be properly controlled to protect the furnace lining.
[0007] The purpose of retaining slag in the present invention is to increase the concentration of SiO2 in the early slag and control the basicity of the slag between 0.8 and 1.3. Its purpose is to control the amount of material added in the early stage and release high concentration of SiO2 to the maximum extent, so as to reduce the amount of lime and magnesium-containing auxiliary materials added in the middle and late stages.
[0008] Step 2: Calculate the total oxygen consumption in the early stage of the current furnace:
[0009] Total oxygen consumption in the early stage = oxygen consumption of silicon and manganese in the current furnace molten iron + oxygen consumption of iron in the early stage + oxygen consumption of phosphorus in the early stage + oxygen consumption of carbon in the early stage = M 铁水质量 ×(Si%×1.14×22.4 / 32+Mn%×0.285×22.4 / 32)+M 铁水质量 ×P%×80 / 62 / 32×22.4×50%+(30%-TFe%)×M 前期渣量 ×16 / 56 / 32×22.4+0.5×W 烟气流量 ×T 供氧时间 ×CO 烟气 %, where M 前期渣量 =M 留渣量 +M 前期添加的造渣量 +M 铁水质量 ×(Si 铁水 %×2.14+Mn 铁水 %×R), TFe% is the total iron content of the upper furnace slag, T 供氧时间 = 2~4 minutes, CO 烟气 %=6~15%;
[0010] In the early stage of smelting, while silicon and manganese are being oxidized, carbon and iron are also being oxidized, but the oxidation rate is significantly lower than that of silicon and manganese. In order to ensure that silicon and manganese are completely oxidized, according to a large number of on-site test data, it is found that when the total iron content in the current slag is about 30%, the oxidation of silicon and manganese is basically completed. At this time, the gun is raised. Due to the low oxidizability of the slag, a large amount of carbon-oxygen reaction has not occurred, the probability of splashing is very low, and a large amount of slag with high SiO2 content can be released. The mechanism of carbon-oxygen reaction is: (FeO) + C = Fe + CO. It can be seen from the reaction formula that in order for the reaction to proceed to the right, there must be a large amount of FeO and a suitable temperature (the above reaction is endothermic). Therefore, if the large amount of FeO can be controlled, the probability of splashing in the early stage can be reduced. The generation of FeO mainly comes from the oxidation of FeO generated by supplying oxygen to the furnace. Therefore, if the oxygen supply time in the furnace is controlled, the carbon-oxygen reaction can be controlled. If the total iron content of the previous slag is 30%, and the total iron content of the upper furnace slag is TFe%, it is considered that the total iron added to the previous slag is FeO, so the oxygen consumption of the iron element in the early stage is (30%-TFe%)×M 前期渣量 ×16 / 56 / 32×22.4, and M 前期渣量 =M 留渣量 +M 前期添加的造渣量 +M 铁水质量 ×(Si 铁水 %×2.14+Mn 铁水%×1.3), the slag-making materials added in the early stage are determined according to the requirements of binary alkalinity and magnesium oxide content in the early stage. The slag-making materials mainly include lime, light-burned dolomite or magnesium balls.
[0011] Due to the slag retention operation, some active calcium oxide and iron oxide remain in the slag of the upper furnace, which meets the conditions for dephosphorization reaction. Through a large number of on-site tests, it is found that more than 50% of the phosphorus element is oxidized into the slag in the early stage to form P2O5. Therefore, the oxygen consumption of phosphorus element in molten iron = M 铁水质量 ×P%×80 / 62 / 32×22.4×50%.
[0012] Due to the slag retention operation, there is about 20% TFe% in the slag of the upper furnace, and the oxidation of iron elements after smelting begins, so the carbon-oxygen reaction is also in progress. The temperature in the furnace is low in the early stage of blowing, and the carbon-oxygen reaction is slow. As the temperature rises, the reaction accelerates. Through field test tracking, it is found that when the carbon monoxide concentration in the converter flue gas reaches more than 15%, the probability of splashing is very high. Therefore, the gun must be lifted when the carbon monoxide concentration is less than 15%. In order to ensure that the oxidation of silicon and manganese elements is completed, it is necessary to consider part of the oxygen consumed for the oxidation of carbon elements, and at the same time consider the lower risk of splashing. According to field tests, the carbon monoxide concentration in the flue gas is about 6-15% after 2-4 minutes of oxygen supply. At this time, the risk of lifting the gun is low. Therefore, the oxygen consumption of carbon elements is calculated when the carbon monoxide concentration in the flue gas reaches 10%. Since the flow rate of the flue gas is known, the total amount of carbon monoxide in the flue gas during 2-4 minutes of blowing can be calculated, and then the consumed oxygen can be calculated. Carbon element oxygen consumption = 0.5×W 烟气流量 ×T 供氧时间 ×CO 烟气 %, where T 供氧时间 = 3 minutes, CO 烟气 %=6~15%, 10% is the best, all are empirical values.
[0013] Therefore, the present invention requires that when an oxygen lance is provided, the oxygen blowing amount is greater than the oxygen consumption of carbon, silicon, manganese and iron elements in the molten iron in the early stage, the total oxygen supply deviation is controlled within 5%, and the flue gas carbon monoxide concentration is less than 15%, so as to avoid splashing.
[0014] Step 3: The initial oxygen supply flow rate is 2.8~3.0m 3 / t·min oxygen is blown into the furnace, and the carbon monoxide concentration in the flue gas is detected at the same time. When the oxygen supply reaches the total oxygen consumption in the early stage or the carbon monoxide concentration is greater than 15%, the oxygen supply is stopped. The main purpose of the low oxygen supply intensity mode of the present invention is to facilitate the rapid formation of slag in the early stage and achieve the purpose of increasing the slag discharge amount.
[0015] Step 4: After stopping the oxygen supply, immediately blow nitrogen into the furnace through the oxygen lance for 40 to 60 seconds, with the nitrogen pressure being 1.0 to 1.3 MPa and the total gas supply being 3 to 4.0 m3 per ton of molten iron. 3 , nitrogen intensity is 3.5~3.8m 3 / t·min. After the gun is lifted, high-pressure nitrogen is supplied to the furnace through the oxygen gun. The high-pressure nitrogen is used to blow nitrogen into the furnace, which can foam the slag and form a large number of bubbles. Due to the low surface tension of the bubbles, the iron beads in the slag can be quickly settled. At the same time, due to the good foaming of the slag, more than 40% of the slag can be effectively discharged, thereby quickly forming slag, and there is no need to rely on manual experience to judge whether foam slag is formed. The purpose of controlling the nitrogen supply time is to avoid too long nitrogen blowing time, excessive temperature loss in the furnace, and a large decrease in slag temperature and reduced fluidity, which affects the slag discharge amount.
[0016] Step 5: After the nitrogen supply to the furnace is completed, the furnace is turned over to discharge the slag, and the slag discharge angle is 87~90 degrees. This can ensure that the slag is fully discharged and prevent the molten iron in the furnace from overflowing.
[0017] Step 6: Continue to supply oxygen to the furnace for blowing after slag discharge. During blowing, the first 40-50% of the total oxygen consumption in the later stage is 2.8-3.0m 3 / t·min oxygen supply intensity, the last 50~60% of the total oxygen consumption in the later period is 3.2~3.4m 3 / t·min oxygen supply intensity until the blowing is completed, the temperature of the blowing end point is preferably 1630~1660℃, which is conducive to preventing rephosphorization. It should be noted that the calculation of the total oxygen consumption of each heat is a prior art, and those skilled in the art can easily obtain it, and the difference between the total oxygen consumption of each heat and the total oxygen consumption in the early stage is the total oxygen consumption in the later stage.
[0018] In the process of supplying oxygen to the furnace, some oxygen will generally escape, and the oxygen utilization coefficient e=0.9~0.95. Therefore, in order to compensate for the part of oxygen escaping in the process of supplying oxygen to the furnace, the above technical solution is further improved: in the third step, the actual required oxygen supply = the total oxygen consumption in the previous stage / e, and the oxygen supply is stopped when the oxygen supply reaches the actual required oxygen supply.
[0019] In order to control the appropriate gun position, which is beneficial to impacting slag and molten iron and quickly forming emulsified slag, the above technical solution is further improved: when blowing nitrogen into the furnace in the fourth step, the height of the oxygen gun nozzle from the molten iron liquid level is 2.0~5.0 meters.
[0020] When the oxygen supply lasts for more than 4 minutes, the temperature of the molten pool continues to rise, and the carbon-oxygen reaction causes a large amount of carbon monoxide to accumulate in the slag, which is easy to cause splashing. Therefore, in order to avoid risks, the above technical solution is further improved as follows: if the oxygen supply time exceeds 4 minutes in the third step, stop the oxygen supply and discharge the slag until the slag in the furnace no longer flows outward, and then blow the remaining oxygen into the furnace again. When discharging the slag, the slag discharge angle is controlled at 87~90 degrees until a small amount of slag in the furnace flows out or no longer flows outward. Since the slag discharge is carried out more than once, the amount of slag in the furnace is discharged in large quantities, and the total amount of slag in the furnace decreases when oxygen is blown again, that is, the total amount of iron oxide in the slag is released in large quantities, and the carbon-oxygen reaction rate decreases when oxygen is blown again. At the same time, the decrease in the total amount of slag reduces the thickness of the slag layer, which is conducive to the discharge of carbon monoxide gas from the slag layer, thereby reducing the risk of splashing.
[0021] The beneficial effects brought by the present invention are as follows: the present invention adopts the mode of retaining slag, and in order to achieve a better dephosphorization effect, part or all of the slag from the previous furnace is retained for the current furnace, and at the same time, the oxygen consumption required for the oxidation of the main elements of carbon, silicon, manganese and iron in the previous molten iron is used, and the carbon monoxide concentration in the flue gas is referred to, and the oxygen supply time is controlled to be 2≤≤4 minutes, as a reference for the early gun lifting, so as to avoid metal splashing caused by late gun lifting. In order to increase the concentration of SiO2 in the early slag, the basicity of the slag is controlled between 1.1 and 1.3, and the purpose is to control the amount of material added in the early stage to release high concentration of SiO2 to the maximum extent. 2, The problem of reducing the amount of lime and magnesium-containing auxiliary materials added in the middle and late stages is achieved. After the gun is lifted, high-pressure nitrogen is used to blow nitrogen into the furnace to foam the slag, without relying on manual experience to judge whether foamed slag is formed. High-pressure nitrogen is supplied to the furnace through an oxygen gun to form a large number of bubbles in the slag. Due to the low surface tension of the bubbles, the purpose of quickly settling the iron beads in the slag is achieved. At the same time, due to the good foaming of the slag, more than 40% of the slag can be effectively discharged. The benefit of the present invention is that it can avoid splashing caused by lifting the gun too late. Since the oxygen supply time to the furnace is controlled in the early stage, the iron oxide content of the slag can be effectively reduced. At the same time, slag bubbles can be formed by the impact of high-pressure nitrogen on the slag, which plays a role in reducing the surface tension of the slag bubbles, so that the iron beads in the slag can be quickly settled in the molten pool, so as to achieve the purpose of separating molten iron from slag, and to achieve the purpose of increasing the slag discharge amount and reducing the loss of metal materials, so that the iron oxide content in the early slag is controlled below 21%, and the average level is about 16%. Since the basicity of the slag was controlled at 1.1~1.3 in the early stage, high-concentration SiO2 slag was released to the maximum extent, so that the subsequent slag basicity was guaranteed, and the converter dephosphorization efficiency reached more than 87%. DETAILED DESCRIPTION
[0022] Embodiment 1
[0023] In this example, the current furnace has 150 tons of molten iron, 20 tons of scrap steel, and a converter flue gas flow rate of 100,000 m 3 / h, the composition of molten iron is shown in Table 1.
[0024] Table 1
[0025] C% Si% <![CDATA[M n %]]> P% S% 4.2% 0.4% 0.3% 0.11% 0.025%
[0026] The slag composition of the upper furnace is shown in Table 2:
[0027] Table 2
[0028] CaO% <![CDATA[SiO2%]]> MgO% MnO% P% TFe% 42% 13.5% 8% 0.3% 0.11% 18.5%
[0029] The control method for converter double slag smelting in this embodiment includes the following steps:
[0030] The first step is to keep part or all of the slag from the previous furnace for the current furnace. According to the silicon content of the molten iron of the current furnace, the binary basicity of the previous slag and the content of magnesium oxide in the previous furnace, lime and / or magnesium-containing auxiliary materials are added as slag-making in the early stage of the current furnace. The amount of slag-making added in the early stage makes the binary basicity R of the slag in the early stage of the current furnace meet 1.1≤R≤1.3 and the content of magnesium oxide is greater than 6%;
[0031] Among them, the amount of slag left in the upper furnace is: M 留渣量 =R×(M 铁水质量 ×Si 铁水 %×2.14) / (CaO 上炉炉渣 %-R×SiO 2上炉炉渣 %); binary basicity R = CaO / SiO2, R value is 1.3 。
[0032] That is, according to the binary basicity of the previous slag of 1.3, the amount of retained slag = 1.3×(150000×0.4%×2.14) / (42%-1.3*13.5%)=7494kg, that is, 7494kg of the slag from the previous furnace will be retained for the current furnace.
[0033] Step 2: Calculate the total oxygen consumption in the early stage of the current furnace:
[0034] Total oxygen consumption in the early stage = oxygen consumption of silicon and manganese in the current furnace molten iron + oxygen consumption of iron in the early stage + oxygen consumption of phosphorus in the early stage + oxygen consumption of carbon in the early stage = M 铁水质量 ×(Si%×1.14×22.4 / 32+Mn%×0.285×22.4 / 32)+M 铁水质量 ×P%×80 / 62 / 32×22.4×50%+(30%-TFe%)×M 前期渣量 ×16 / 56 / 32×22.4+0.5×W 烟气流量 ×T 供氧时间 ×CO烟气 %, where M 前期渣量 =M 留渣量 +M 前期添加的造渣量 +M 铁水质量 ×(Si 铁水 %×2.14+Mn 铁水 %×R), TFe% is the total iron content of the upper furnace slag, T 供氧时间 = 3 minutes, CO 烟气 %=10%, R=1.3.
[0035] First, calculate whether it is necessary to add slag-making materials in the early stage. The amount of 150 tons of converter slag is about 80kg / t~100kg / t, so the total slag produced is about 12000kg~150000kg, which can fully meet the slag retention of 7494kg. Therefore, there is no need to add lime to meet the binary basicity requirement of R=1.3. The amount of slag in the early stage = 7494 + slag-making materials added in the early stage + 150000×(0.4%×2.14+0.3%×1.3)=9363+ slag-making materials added in the early stage. Calculate whether the magnesium oxide in the early slag is greater than 6% without adding magnesium-containing auxiliary materials. The magnesium oxide content in the early slag = 7494×8% / 9363×100%=6.4%. Therefore, there is no need to add lime or magnesium-containing auxiliary materials in the early stage, so the amount of slag in the early stage = 9363kg.
[0036] The oxygen consumption of silicon and manganese in the current batch of molten iron = 150000 × (0.4% × 1.14 × 22.4 / 32 + 0.3% × 0.285 × 22.4 / 32) = 568.6m 3 .
[0037] Initial iron oxygen consumption = (30%-18.5%) × 9363 × 16 / 56 / 32 × 22.4 = 215.3 m 3 .
[0038] Early stage phosphorus oxygen consumption = M 铁水质量 ×P%×80 / 62 / 32×22.4×50%=150000×0.11×%80 / 62 / 32×22.4×50%80 / 62 / 32×22.4×50%80 / 62 / 32×22.4×50%=77m 3 .
[0039] Initial carbon oxygen consumption = 0.5×100000×3 / 60×10%=250m 3 The oxygen supply time is calculated as an average of 3 minutes, and the carbon monoxide concentration is calculated as 10%.
[0040] Therefore, the total oxygen consumption in the early stage = 568.6 + 215.3 + 77 + 250 = 1110.9m 3 .
[0041] Step 3: Control the initial oxygen flow rate to 2.8~3.0m 3 / t·min oxygen is blown into the furnace and the carbon monoxide concentration in the flue gas is detected at the same time. When the oxygen supply reaches the previous total oxygen consumption or the carbon monoxide concentration is greater than 15%, the oxygen supply is stopped.
[0042] According to the smelting requirements, 20 tons of scrap steel and 150 tons of molten iron were added to the furnace. 3 / h(3.0m 3 / t·min) to blow oxygen into the furnace, and the oxygen supply gun position is carried out according to the normal blowing gun position. When the oxygen supply is greater than 1100.9m 3 When the oxygen supply is stopped, the oxygen supply time = 1110.9×60 / 28000 = 2.38 minutes.
[0043] Step 4: After stopping the oxygen supply, immediately blow nitrogen into the furnace through the oxygen lance for 40 to 60 seconds, preferably 50 seconds, with the nitrogen pressure at 1.0 to 1.3 MPa and the total gas supply at 3 to 4.0 m3 per ton of molten iron. 3 , nitrogen intensity is 3.5~3.8m 3 / t·min. The purpose of controlling the nitrogen supply time is to avoid too long nitrogen blowing time, excessive temperature loss in the furnace, too much drop in slag temperature and reduced fluidity, which affects the slag discharge amount.
[0044] When blowing nitrogen into the furnace, the gun position is controlled so that the oxygen gun nozzle is 2.0~5.0 meters away from the molten iron liquid surface. Controlling the appropriate gun position is beneficial to impacting the slag and molten iron and quickly forming emulsified slag.
[0045] Step 5. After the nitrogen supply to the furnace is completed, the furnace is turned over to discharge the slag. The slag discharge angle is 87~90 degrees to ensure sufficient slag discharge while preventing the molten iron in the furnace from overflowing.
[0046] Step 6: Continue to supply oxygen to the furnace for blowing after slag discharge. During blowing, the first 40-50% of the total oxygen consumption in the later stage is 2.8-3.0m 3 / t·min oxygen supply intensity is conducive to slag slag, the latter 50%~60% of the total oxygen consumption in the later period is 3.2~3.4 m 3 / t·min oxygen supply intensity until the blowing is completed, the terminal temperature is best controlled at 1630~1660℃, which is beneficial to prevent rephosphorization.
[0047] Through the above operation, there is no splashing when lifting the gun, the smelting process is stable, the phosphorus content of the converter is 0.012% on time, the dephosphorization efficiency is 89%, and the composition of the slag obtained during the early slag pouring is shown in Table 3 below:
[0048] Table 3
[0049] Serial number TFe% Cao% <![CDATA[SiO2%]]> Binary Alkalinity 1 17.6 29.45 23 1.280
[0050] The composition data of slag during the early stage of slag discharge of some furnaces on site are shown in Table 4:
[0051] Table 4
[0052] Serial number TFe% CaO% <![CDATA[SiO2%]]> Binary Alkalinity 1 16.49 31.5 33.92 0.929 2 15.7 32 33.83 0.946 3 12.44 35.84 32.57 1.100 4 14.42 35.36 31.2 1.133 5 18.5 33.75 29.53 1.143 6 9.84 36.86 31.44 1.172 7 17.87 33.37 27.49 1.214 8 12.41 36.3 29.58 1.227 9 19.53 34.17 27.42 1.246 10 17.37 35.07 27.82 1.261 11 12.72 37.05 28.36 1.306 12 13.88 33 25.5 1.294
[0053] The present embodiment can also be improved as follows: In the process of supplying oxygen to the furnace, some oxygen generally escapes, and the oxygen utilization coefficient e=0.9~0.95. Therefore, in order to compensate for the oxygen that escapes during the process of supplying oxygen to the furnace, the actual oxygen supply required in the third step = the total oxygen consumption in the previous period / e (in this example, e is 0.9). When the oxygen supply reaches the actual required oxygen supply, the oxygen supply is stopped. The actual required oxygen supply = 1110.9 / 0.9 = 1234m 3 When the oxygen supply reaches the actual required oxygen supply 1234m 3 Stop oxygen supply, oxygen supply time = 1234 × 60 / 28000 = 2.64 minutes. In addition, the deviation of oxygen supply is usually controlled within 5%, so the maximum oxygen supply time is 2.77 minutes, that is, the actual oxygen supply time is controlled within 2.64~2.77 minutes. In this way, silicon and manganese elements can be completely oxidized while avoiding splashing.
[0054] The present invention is not limited to the specific technical solutions described in the above embodiments. In addition to the above embodiments, the present invention may also have other implementation modes. For those skilled in the art, any technical solutions formed by any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A control method for converter double slag smelting, The following steps are involved: The first step is to leave part or all of the slag from the previous furnace for the current furnace. According to the silicon content of the molten iron of the current furnace, the binary basicity of the slag in the previous furnace and the content of magnesium oxide in the previous furnace, lime and / or magnesium-containing auxiliary materials are added as slag-making materials in the early stage of the current furnace. The amount of slag-making added in the early stage makes the binary basicity R of the slag in the early stage of the current furnace meet 1≤R≤1.3 and the content of magnesium oxide is greater than 6%; Among them, the amount of slag left in the upper furnace is: M 留渣量 =R×(M 铁水质量 ×Si 铁水 %×2.14) / (CaO 上炉炉渣 %-R×SiO 2上炉炉渣 %), Where: M 留渣量 The unit is kg; M 铁水质量 The unit is kg; Si 铁水 % is the percentage of Si in the current batch of molten iron; CaO 上炉炉渣 % is the percentage of CaO in the upper furnace slag; SiO 2上炉炉渣 % is SiO in the upper furnace slag 2 The percentage content of Step 2: Calculate the total oxygen consumption in the early stage of the current furnace: Total oxygen consumption in the early stage = oxygen consumption of silicon and manganese in the current furnace molten iron + oxygen consumption of iron in the early stage + oxygen consumption of phosphorus in the early stage + oxygen consumption of carbon in the early stage = M 铁水质量 ×(Si 铁水 %×1.14×22.4 / 32+Mn 铁水 %×0.285×22.4 / 32)+M 铁水质量 ×P 铁水 %×80 / 62 / 32×22.4×50%+(30%-TFe 上炉炉渣 %)×M 前期渣量 ×16 / 56 / 32×22.4+0.5×W 烟气流量 ×T 供氧时间 ×CO 烟气 %, where M 前期渣量 =M 留渣量 +M 前期添加的造渣量 +M 铁水质量 ×(Si 铁水 %×2.14+Mn 铁水 % × R); Where: Mn 铁水 % is the percentage of Mn in the current batch of molten iron; P 铁水 % is the percentage of P in the current batch of molten iron; TFe 上炉炉渣 % is the percentage of total iron in the upper furnace slag, T 供氧时间 = 2~4 minutes, CO 烟气 %=6~15%; W 烟气流量 The unit is m 3 / h,M 前期渣量 、M 前期添加的造渣量 The unit of the total oxygen consumption in the early stage is m 3 ; The unit of oxygen consumption of silicon and manganese in the current batch of molten iron is m 3 ; The unit of initial iron oxygen consumption is m 3 ; The unit of oxygen consumption of phosphorus in the early stage is m 3 ; The unit of initial carbon oxygen consumption is m 3 ; Step 3: Control the initial oxygen flow rate to 2.8~3.0m 3 / t·min oxygen is blown into the furnace, and the carbon monoxide concentration in the flue gas is detected at the same time. When the oxygen supply reaches the total oxygen consumption in the previous period or the carbon monoxide concentration is greater than 15%, the oxygen supply is stopped; Step 4: After stopping the oxygen supply, immediately blow nitrogen into the furnace through the oxygen lance for 40 to 60 seconds, with the nitrogen pressure being 1.0 to 1.3 MPa and the total gas supply being 3 to 4.0 m3 per ton of molten iron. 3 , nitrogen intensity is 3.5~3.8m 3 / t·min; Step 5: After the nitrogen supply to the furnace is completed, the furnace is turned over and the slag is discharged. The slag discharge angle is 87~90 degrees; Step 6: Continue to supply oxygen to the furnace for blowing after slag discharge. During blowing, the first 40-50% of the total oxygen consumption in the later stage is 2.8-3.0m 3 / t·min oxygen supply intensity, the last 50~60% of the total oxygen consumption in the later period is 3.2~3.4 m 3 Oxygen is supplied at an intensity of / t·min until the blowing is completed.
2. The control method for converter double slag smelting according to claim 1, Features: In the third step, some oxygen will escape when supplying oxygen to the furnace. The oxygen utilization coefficient is e=0.9~0.
95. The actual required oxygen supply = the total oxygen consumption in the previous stage / e. When the oxygen supply reaches the actual required oxygen supply, stop supplying oxygen.
3. The control method for converter double slag smelting according to claim 1, Features: In the third step, if the oxygen supply time exceeds 4 minutes, the oxygen supply is stopped and the slag is released until the slag in the furnace no longer flows outward, and then the remaining oxygen is blown into the furnace again.
4. The control method for converter double slag smelting according to claim 1, Features: In the fourth step, when blowing nitrogen into the furnace, the height of the oxygen lance nozzle from the molten iron surface is 2.0~5.0 meters.
5. The control method for converter double slag smelting according to claim 4, Features: In the sixth step, the temperature at the end of blowing is 1630~1660℃.