A high-power flip-chip LED and its fabrication method

By using the Ag reflective layer and Al layer to form an ODR structure in a high-power flip LED chip, the problems of low reflectivity and light output efficiency are solved, and efficient reflectivity and brightness are achieved, avoiding the fall of the Ag layer and ensuring that The stability and efficient light emission of the chip.

CN110491981BActive Publication Date: 2024-11-29FOSHAN NATIONSTAR SEMICONDUCTOR CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201910746741.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-08-14
Publication Date
2024-11-29
Estimated Expiration
2039-08-14

AI Technical Summary

Technical Problem

Large-size high-power flip LED chips have core fragmentation due to excessive stress during cutting and sorting, and the Ag layer of the ODR system composed of SiO2/Ag is problematic, and the reflectivity and light output efficiency are low.

Method used

An ODR structure is formed by using the Ag reflective layer and the Al layer to fill the area that the Ag reflective layer cannot reflect through the insulating layer, increase the reflection efficiency, and improve adhesion by optimizing the thickness ratio of the insulating layer and the Al layer to prevent the Ag layer from falling off.

Benefits of technology

The reflectivity and light output efficiency of the chip are improved, the Ag layer is avoided, the brightness and stability of the chip are enhanced, cost-saving and maximum light output efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110491981B_ABST
    Figure CN110491981B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-power flip-chip LED chip and a manufacturing method thereof, wherein the chip comprises a substrate, an epitaxial layer, an Ag reflective layer, an insulating layer, an Al layer, a first electrode and a second electrode, wherein the insulating layer and the Al layer form an ODR structure. The present invention utilizes the Al layer to fill the non-reflective area of ​​the Ag reflective layer, thereby increasing the overall reflection efficiency of the chip and improving the light extraction efficiency of the chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of light emitting diodes, and in particular to a high-power flip-chip LED chip and a manufacturing method thereof. Background Art

[0002] In flip-chip LED chips, Ag reflective structures and DBR reflective structures are commonly used to improve light extraction efficiency. Among them, the DBR reflective structure is generally formed by alternating two materials with different refractive indices. The manufacturing process is complicated and time-consuming, and the reflectivity is not as good as the Ag reflective structure. However, the Ag reflective structure is easy to oxidize and needs to be protected by another layer of other metals. Therefore, there is a part of the area between the Ag reflective structure and the N-type layer that does not reflect light, thereby reducing the reflectivity and light extraction efficiency of the chip.

[0003] Patent publication number CN106098893A discloses a simple ODR structure flip-chip gallium nitride-based light-emitting diode and a preparation method thereof. The patent uses Ag pads and DBR structures to form an ODR structure to improve the reflectivity of incident light at different angles.

[0004] If a large-sized high-power flip-chip LED chip adopts a DBR reflective structure, the core particles will break due to excessive stress during chip cutting and sorting. In addition, it has been verified that the Ag layer will fall off in the ODR system composed of SiO2 / Ag, and the bonding strength between the two is poor. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a high-power flip-chip LED chip and a manufacturing method thereof, forming an ODR structure to improve the light extraction efficiency of the flip-chip LED chip.

[0006] In order to solve the above technical problems, the present invention provides a high-power flip-chip LED chip, comprising a substrate, an epitaxial layer, an Ag reflective layer, an insulating layer, an Al layer, a first electrode and a second electrode, wherein the insulating layer and the Al layer form an ODR structure;

[0007] The epitaxial layer is provided with a first hole, the Ag reflective layer is disposed on the epitaxial layer and is provided with a second hole, the second hole is connected to the first hole, and the diameter of the second hole is greater than the diameter of the first hole;

[0008] The insulating layer is arranged on the Ag reflective layer and filled in the second hole and the first hole, the insulating layer is provided with a third hole and a fourth hole, the third hole is located in the first hole and the second hole, and the diameter of the third hole is smaller than the diameter of the first hole;

[0009] The Al layer is disposed on the insulating layer, and the Al layer is located in a region between the third hole and the Ag reflective layer;

[0010] The first electrode is disposed in the third hole, and the second electrode is disposed in the fourth hole.

[0011] As an improvement of the above solution, the epitaxial layer includes a first semiconductor layer, an active layer and a second semiconductor layer which are sequentially arranged on the substrate, and the first hole penetrates the second semiconductor layer and the active layer and extends to the first semiconductor layer.

[0012] As an improvement of the above solution, the second hole penetrates the Ag reflective layer, and the diameter of the second hole is 5% to 10% larger than the diameter of the first hole.

[0013] As an improvement of the above solution, the thickness of the insulating layer>the thickness of the Ag reflective layer>the thickness of the Al layer.

[0014] As an improvement of the above solution, the thickness of the insulating layer is 3 to 5 times greater than the thickness of the Ag reflective layer, and the thickness of the Ag reflective layer is 3% to 10% greater than the thickness of the Al layer.

[0015] As an improvement of the above solution, the thickness of the insulating layer is 4000 to 6000 angstroms, the thickness of the Ag reflective layer is 1000 to 2000 angstroms, and the thickness of the Al layer is 1000 to 2000 angstroms.

[0016] As an improvement of the above solution, the insulating layer is made of SiO2, Si3N4, SiO x N y The Al layer is made of one or more of the following:

[0017] As an improvement of the above solution, the insulating layer is made of SiO2, and the Al layer is made of aluminum.

[0018] As an improvement of the above solution, the first electrode extends from the third hole to the Al layer and the insulating layer, and a passivation layer is provided between the first electrode and the second electrode, and the two are insulated from each other.

[0019] Accordingly, the present invention also provides a method for manufacturing a high-power flip-chip LED chip, comprising the following steps:

[0020] 1. forming an epitaxial layer on a substrate, and etching the epitaxial layer to form a first hole;

[0021] 2. forming an Ag reflective layer on the second semiconductor layer, and etching the Ag reflective layer to form a second hole;

[0022] 3. forming an insulating layer on the Ag reflective layer and in the second hole and the first hole, and etching the insulating layer to form a third hole and a fourth hole;

[0023] 4. forming an Al layer on the insulating layer in a region between the third hole and the Ag reflective layer;

[0024] 5. Form a first electrode in the third hole and form a second electrode in the fourth hole.

[0025] The implementation of the present invention has the following beneficial effects:

[0026] The present invention provides a high-power flip-chip LED chip, comprising a substrate, an epitaxial layer, an Ag reflective layer, an insulating layer, an Al layer, a first electrode and a second electrode, wherein the insulating layer and the Al layer form an ODR structure;

[0027] The present invention utilizes the Al layer to fill the non-reflective area of ​​the Ag reflective layer, thereby increasing the overall reflection efficiency of the chip and improving the light extraction efficiency of the chip.

[0028] The present invention adopts an Al layer and a SiO2 insulating layer as the ODR structure of the present invention. Since Al and SiO2 have good adhesion, they are not prone to falling off.

[0029] The present invention further limits the position and size of the Al layer, thereby saving costs and maximizing the light extraction efficiency of the chip. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a schematic structural diagram of an LED chip according to an embodiment of the present invention;

[0031] Figure 2 is a schematic diagram of the structure of the LED chip of Embodiment 2 of the present invention;

[0032] Figure 3a is a schematic structural diagram of an LED chip after a first hole is formed in a first embodiment of the present invention;

[0033] Figure 3b is a schematic structural diagram of an LED chip after a second hole is formed in a first embodiment of the present invention;

[0034] Figure 3c is a schematic diagram of the structure of the LED chip after the third hole and the fourth hole are formed in the first embodiment of the present invention;

[0035] Figure 3d It is a schematic diagram of the structure of the LED chip after the Al layer is formed in the first embodiment of the present invention. DETAILED DESCRIPTION

[0036] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.

[0037] See also Figure 1The present invention provides a large-sized high-power flip-chip LED chip, comprising a substrate 10, an epitaxial layer, an Ag reflective layer 30, an insulating layer 40, an Al layer 50, a first electrode 61 and a second electrode (not shown in the figure). The Al layer 50 and the insulating layer 40 form an ODR structure;

[0038] The epitaxial layer includes a first semiconductor layer 21, an active layer 22, a second semiconductor layer 23 and a first hole which are sequentially arranged on the substrate 10. Specifically, the first hole penetrates the second semiconductor layer 23 and the active layer 22 and extends to the first semiconductor layer 21. Preferably, the first hole is located at the geometric center of the epitaxial layer, but is not limited thereto. In other embodiments of the application, a plurality of the first holes may be provided.

[0039] The Ag reflective layer 30 is made of silver and is disposed on the second semiconductor layer 23. The Ag reflective layer 30 is used to reflect the light emitted by the active layer 22 toward the substrate side to improve the light extraction efficiency of the chip.

[0040] The Ag reflective layer 30 of the present invention is provided with a second hole, and the second hole is located above the first hole and communicated with the first hole.

[0041] It should be noted that the diameter and number of the first hole, i.e. the MESA aperture, have an impact on the light emission efficiency and current distribution. Since part of the metal in the Ag reflective layer falls into the quantum well, it will cause a short circuit and burn the core particles, so the aperture of the second hole should be larger than that of the first hole.

[0042] Since the aperture of the second hole is larger than that of the first hole, the larger the aperture of the first hole, the smaller the area of ​​the Ag reflective layer and the lower the reflectivity. Preferably, the diameter of the first hole is 40 to 60 μm. The diameter of the second hole is 5 to 10% larger than that of the first hole.

[0043] The insulating layer 40 is made of SiO2, Si3N4, SiO x N y Preferably, the insulating layer 40 is made of SiO2. The insulating layer 40 of the present invention is arranged on the Ag reflective layer 30 and filled in the first hole and the second hole. Specifically, the insulating layer 40 located in the first hole and the second hole is provided with a third hole. The third hole is located at the geometric center of the first hole and the second hole, but is not limited thereto.

[0044] The Al layer 50 is made of aluminum and is disposed on the insulating layer 40. It should be noted that in the existing flip-chip LED chip, the insulating layer 40 is used to protect the first hole and the Ag reflective layer; the Al layer 50 is used to reflect the light emitted by the active layer 22 toward the substrate side to improve the light extraction efficiency of the chip.

[0045] The main function of the Al layer 50 of the present invention is to fill the non-reflective area of ​​the Ag reflective layer 30 (the area of ​​the second hole) and increase the reflection efficiency. Among them, the adhesion between Ag and SiO2 is not as good as that between Al and SiO2. The aperture of the Ag reflective layer should be made larger than the aperture of the MESA as much as possible to prevent Ag from falling off to the quantum well area and causing leakage. However, such a design will reduce the area of ​​a part of the metal reflective layer, so that the brightness of the chip cannot be well improved. The ODR structure of the present invention can just make up for this.

[0046] In order to further improve the adhesion between the Al layer and the insulating layer, and the reflection efficiency between the Al layer and the Ag reflective layer, a certain proportional relationship is maintained among the insulating layer, the Ag reflective layer and the Al layer. Preferably, the thickness of the insulating layer is 3 to 5 times greater than that of the Ag reflective layer, and the thickness of the Ag reflective layer is 3% to 10% greater than that of the Al layer.

[0047] If the thickness of the insulating layer exceeds the above range compared to the thickness of the Al layer, the reflection efficiency of the Al layer will be affected; if it is less than the above range, the adhesion of the two will be affected. Furthermore, if the thickness ratio of the Al layer and the Ag reflective layer is less than or greater than the above range, the light uniformity of the chip will be affected.

[0048] The Al layer 50 and the insulating layer 40 of the present invention form an ODR structure for reflecting the light emitted by the active layer 22 toward the substrate side to improve the light extraction efficiency of the chip. The ODR structure of the present invention can increase the reflectivity to more than 97%, and the brightness of the chip is increased by about 1.5%.

[0049] The reflectivity of the ODR structure is not only affected by the material and structure, but also by the thickness. In order to improve the reflectivity of the ODR structure and the overall light extraction efficiency of the chip, the present invention limits the thickness of the ODR structure according to the material properties of the ODR structure and the Ag reflective layer. Preferably, the thickness of the insulating layer 40> the thickness of the Ag reflective layer 30> the thickness of the Al layer 50. Specifically, the thickness of the insulating layer is 4000-6000 angstroms, the thickness of the Ag reflective layer is 1000-2000 angstroms, and the thickness of the Al layer is 1000-2000 angstroms. Experiments have shown that the reflectivity of the metal reflective layer increases first and then decreases with the change of film thickness. The reflectivity of the Al layer and the Ag reflective layer is the largest when the thickness is 1000-2000 angstroms, and SiO2 has light absorption. Too thick thickness will reduce the brightness, and too thin film thickness will cause leakage. The best effect is between 4000 and 6000 angstroms.

[0050] The first electrode 61 of the present invention is filled in the third hole and is conductively connected to the first semiconductor layer 21. Preferably, the first electrode 61 extends from the third hole to the insulating layer 40. The second electrode is conductively connected to the second semiconductor layer 23, and the first electrode and the second electrode are insulated from each other.

[0051] In order to ensure that the first electrode and the second insulation are insulated from each other, the chip of the present invention further includes a passivation layer, which is made of an insulating material and is disposed on the first electrode. The second electrode is disposed on the passivation layer and is conductively connected to the second semiconductor layer. Specifically, a bare area is provided on the passivation layer to expose the first electrode. Preferably, the second electrode of the present invention penetrates the passivation layer and the insulation layer and is conductively connected to the Ag reflective layer.

[0052] See also Figure 2 As another preferred embodiment of the present invention, a large-sized high-power flip-chip LED chip provided by the present invention further includes a current spreading layer 24, which is disposed between the second semiconductor layer 23 and the Ag reflective layer 30. The current spreading layer is provided with a fourth hole, wherein the fourth hole is connected to the first hole and the second hole, and the diameter of the fourth hole is between the first hole and the second hole.

[0053] Accordingly, the present invention also provides a method for manufacturing a large-sized high-power flip-chip LED chip, comprising the following steps:

[0054] 1. forming an epitaxial layer and a first hole on a substrate;

[0055] See also Figure 3a An epitaxial layer is formed on the substrate 10 by using an MOCVD process. The epitaxial layer includes a first semiconductor layer 21, an active layer 22 and a second semiconductor layer 23 which are sequentially arranged on the substrate 10.

[0056] The epitaxial layer is etched to form a first hole 24 that penetrates the second semiconductor layer 23 and the active layer 22 and extends to the first semiconductor layer 21. Preferably, the first hole is located at the geometric center of the epitaxial layer, but is not limited thereto. In other embodiments of the application, a plurality of the first holes may be provided.

[0057] 2. forming an Ag reflective layer and a second hole on the second semiconductor layer;

[0058] See also Figure 3b , a Ag reflective layer 30 is formed on the second semiconductor layer 23 by magnetron sputtering or evaporation.

[0059] The Ag reflective layer 30 is etched to form a second hole 31, which is located above the first hole 24 and communicates with the first hole 24. Preferably, the diameter of the second hole 31 is greater than the diameter of the first hole 24. More preferably, the diameter of the second hole is 5-10% greater than the diameter of the first hole.

[0060] 3. forming an insulating layer and a third hole;

[0061] See also Figure 3c An insulating layer 40 is formed on the Ag reflective layer 30 , and the insulating layer 40 extends along the Ag reflective layer 30 into the second hole 31 and the first hole 23 .

[0062] The insulating layer 40 is etched to expose the first semiconductor layer 21 to form a third hole 41, and the Ag reflective layer 30 is exposed to form a fourth hole (not shown in the figure), wherein the third hole 41 is located inside the first hole 24 and the second hole 31, and the diameter of the third hole 41 is smaller than the diameter of the first hole 24. In addition, the sidewalls of the third hole 41 are all left with an insulating layer.

[0063] 4. forming an Al layer on the insulating layer;

[0064] See also Figure 3d , an Al layer 50 is formed on the insulating layer 40 . Preferably, the Al layer 50 is located in a region between the third hole 41 and the Ag reflective layer 30 .

[0065] 5. forming a first electrode and a second electrode;

[0066] See also Figure 1 , metal is deposited in the third hole 41 to form the first electrode 61 , and metal is deposited in the fourth hole to form the second electrode (not shown in the figure). Preferably, the first electrode 61 can extend from the third hole 41 to the insulating layer 40 .

[0067] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A high-power flip-chip LED chip, characterized in that: It includes a substrate, an epitaxial layer, an Ag reflective layer, an insulating layer, an Al layer, a first electrode and a second electrode, wherein the insulating layer and the Al layer form an ODR structure; The epitaxial layer is provided with a first hole, the Ag reflective layer is disposed on the epitaxial layer and is provided with a second hole, the second hole is connected to the first hole, and the diameter of the second hole is greater than the diameter of the first hole; The insulating layer is arranged on the Ag reflective layer and filled in the second hole and the first hole, the insulating layer is provided with a third hole and a fourth hole, the third hole is located in the first hole and the second hole, and the diameter of the third hole is smaller than the diameter of the first hole; The insulating layer includes SiO2, the Al layer is arranged on the upper surface of the SiO2, and the Al layer is located in the area between the third hole and the Ag reflective layer; The first electrode is disposed in the third hole, and the second electrode is disposed in the fourth hole; The second hole penetrates the Ag reflective layer, and the diameter of the second hole is 5% to 10% larger than the diameter of the first hole. The epitaxial layer includes a first semiconductor layer, an active layer and a second semiconductor layer which are sequentially arranged on a substrate, and the first hole penetrates the second semiconductor layer and the active layer and extends to the first semiconductor layer.

2. The high-power flip-chip LED chip according to claim 1, characterized in that: The thickness of the insulating layer>the thickness of the Ag reflective layer>the thickness of the Al layer.

3. The high-power flip-chip LED chip according to claim 2, characterized in that: The thickness of the insulating layer is 3 to 5 times greater than that of the Ag reflective layer, and the thickness of the Ag reflective layer is 3% to 10% greater than that of the Al layer.

4. The high-power flip-chip LED chip according to claim 1, characterized in that: The thickness of the insulating layer is 4000-6000 angstroms, the thickness of the Ag reflective layer is 1000-2000 angstroms, and the thickness of the Al layer is 1000-2000 angstroms.

5. The high-power flip-chip LED chip according to claim 1, characterized in that: The insulating layer is made of SiO2, Si3N4, SiO x N y Made of several kinds.

6. The high-power flip-chip LED chip according to claim 1, characterized in that: The insulating layer is made of SiO2.

7. The high-power flip-chip LED chip according to claim 1, characterized in that: The first electrode extends from the third hole to the Al layer and the insulating layer. A passivation layer is provided between the first electrode and the second electrode, and the two are insulated from each other.

8. A method for manufacturing a high-power flip-chip LED chip according to any one of claims 1 to 7, characterized in that: The following steps are involved:

1. forming an epitaxial layer on a substrate, and etching the epitaxial layer to form a first hole; 2. forming an Ag reflective layer on the second semiconductor layer, and etching the Ag reflective layer to form a second hole; 3. forming an insulating layer on the Ag reflective layer and in the second hole and the first hole, and etching the insulating layer to form a third hole and a fourth hole; 4. forming an Al layer on the insulating layer in a region between the third hole and the Ag reflective layer; 5. Form a first electrode in the third hole and form a second electrode in the fourth hole.

Citation Information

Patent Citations

  • Inverted gallium nitride-based light-emitting diode with simple ODR structure and preparation method of inverted gallium nitride-based light-emitting diode

    CN106098893A

  • Light emitting diode flip chip for improving light-out rate and preparation method thereof

    CN103682004A

  • Fabrication method of novel high-voltage LED

    CN105552180A

  • High-power flip LED chip

    CN210379104U