A cyclic online grinding and dressing method for vitrified bonded CBN grinding wheels
Through the circulating grinding and online dressing method of the ceramic bonding agent CBN grinding wheel, the grinding wheel is trimmed by mixing abrasives with two-way motor and coolant, which solves the cumbersome problem of CBN grinding wheel dressing, and achieves efficient and uniform grinding wheel dressing effect and improves workpieces Quality and grinding performance.
Patent Information
- Application Number
- CN201910762801.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-08-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2039-08-19
AI Technical Summary
The dressing process of existing CBN grinding wheels is cumbersome and cannot be achieved online dressing, resulting in unqualified workpiece quality and degradation of grinding performance.
The cyclic grinding and online dressing method of ceramic bonding agent CBN grinding wheel is used to determine the dressing time through external online measurement and data processing. The mixing abrasive of the grinding wheel is used to perform online dressing of the grinding wheel with a mixed dressing of the two-way motor and coolant. The hardness of the dressing abrasive is lower than that of the CBN grinding wheel. Grain hardness to avoid physical and mechanical damage to abrasive particles.
It realizes efficient online dressing of CBN grinding wheels, improves grinding accuracy and dressing efficiency, has good height consistency after trimming, has small consumption, is uniform in finishing, and can operate circulating.
Smart Images

Figure CN110576395B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for dressing a grinding wheel, in particular to a cyclic grinding and online dressing method for a CBN grinding wheel, and belongs to the field of precision machining. Background Art
[0002] CBN grinding wheels have excellent grinding performance and are widely used in the processing of difficult-to-process materials.
[0003] When CBN grinding wheel is used to process workpieces on CNC grinding machines, the shaping of the workpiece depends on the shape of the grinding wheel. After a period of use, the abrasive grains of the grinding wheel will gradually become blunt and not sharp, and different degrees of wear will occur during the grinding process, resulting in unqualified workpiece quality or even burn damage after grinding. Effective dressing of the grinding wheel is the prerequisite for ensuring high-quality processing. The grinding wheel should be shaped and trimmed in time, otherwise the workpiece may have a significant error, and in more serious cases, it will be scrapped.
[0004] At present, the dressing of grinding wheels mainly adopts the following methods:
[0005] 1. Diamond pen dressing method. It is used to dress resin-bonded super-hard abrasive grinding wheels. The grinding wheel should rotate at a low speed during dressing; otherwise, the dressing effect will be poor and the diamond pen will wear out quickly. The surface of the grinding wheel dressed by this method is smoother, the grinding performance is poor, and the shape and size accuracy are low. Therefore, this method is only used when there are no other dressing conditions. This method requires a feed base to be specially set on the grinder, a grinding wheel dressing frame to be set on the feed base, and a diamond pen to be installed on the grinding wheel dressing frame. When the grinding wheel needs to be dressed, the relative position of the feed base and the base, as well as the relative position of the grinding wheel dressing frame and the feed base need to be adjusted. The adjustment is relatively complicated, the dressing effect is unstable, and the versatility is poor.
[0006] 2. Grinding and shaping method. This method can also be used for sharpening and is a commonly used dressing method. CBN grinding wheels can be dressed with silicon carbide, corundum, and oilstone, and can also be dressed with power-driven diamond, silicon carbide or corundum grinding wheels. When ordinary abrasive grinding wheels are used as dressing wheels, the shaping accuracy is slightly poor, and the grinding performance of the dressed grinding wheels is good. It is suitable for dressing of grinding wheels with low requirements for profile accuracy or requirements for grinding ability. When diamond grinding wheels are used as dressing wheels, the shaping accuracy is good, but the grinding ability of the dressed grinding wheels is poor, so it is only used for dressing of grinding wheels with high requirements for profile accuracy. In order to improve the grinding ability, both can be used, that is, the diamond grinding wheel is used for shaping and then the ordinary abrasive grinding wheel is used for dressing. Moreover, when dressing, this method needs to remove the CBN grinding wheel and reinstall it on the cylindrical grinder or a special dressing machine for dressing, and it cannot be dressed online. In general, the dressing process of existing CBN grinding wheels is cumbersome and cannot be realized online.
[0007] 3. Soft steel grinding and dressing method. Soft steel grinding and shaping can also be sharpened. Since a lot of abrasive particles fall off during shaping, this method is not suitable for dressing grinding wheels with high surface accuracy requirements. There are two soft steel grinding methods: single roller method and double roller method. The double roller method uses two soft steel rollers. During dressing, the two rollers have the same direction but different speeds. If the linear speed of the grinding wheel to be dressed is Vsd, then the linear speed of one soft steel roller is Vsd+V, and the other is Vsd-V. Therefore, there are two dressing forces of equal size and opposite direction in the tangential direction of the grinding wheel to be dressed. In this way, the grinding wheel to be dressed will not generate additional interference torque, which can ensure the smooth shaping process and improve the shaping quality. Summary of the invention
[0008] The purpose of the present invention is to reduce ineffective processing time, improve grinding accuracy, and provide a cyclic grinding online dressing method for a CBN grinding wheel, thereby solving the problem that the dressing process of the grinding wheel is complicated and online dressing cannot be achieved.
[0009] To achieve the above object, the technical solution of the present invention is implemented in this way, based on using a grinding wheel dresser, judging the working state of the grinding wheel through external online measurement of the workpiece and data processing, and determining the dressing curve of the grinding wheel to determine the dressing time of the CBN grinding wheel, the technical solution adopted includes the following steps:
[0010] A method for cyclic online grinding and dressing of a ceramic bond CBN grinding wheel, wherein a bidirectional motor is arranged on a turntable, CBN grinding wheels are fixed at both ends of the bidirectional motor, the CBN grinding wheel at one end processes a workpiece, and the CBN grinding wheel at the other end is dressed; when the machining grinding wheel needs to be dressed, the turntable is rotated to exchange the machining CBN grinding wheel with the dressed CBN grinding wheel; the grinding wheel dressing method is: the coolant introduced into the grinding part is mixed with a dressing abrasive, and the dressing abrasive can be well embedded in the binder of the CBN grinding wheel under the driving action of the external radial grinding pressure and the coolant, so that the binder is broken and the ground CBN abrasive particles fall off, thereby realizing the online dressing of the CBN grinding wheel. The coolant can be a commercially available grinding fluid.
[0011] The hardness of the dressing abrasive should be lower than the hardness of the abrasive grains of the CBN grinding wheel, and the hardness of the dressing abrasive should be higher than the hardness of the vitrified bond; this is conducive to breaking the bond of the CBN grinding wheel and avoiding physical and mechanical damage to the abrasive grains in the CBN grinding wheel.
[0012] The material of the dressing abrasive can be selected from at least one of corundum and silicon carbide.
[0013] Silicon carbide can be green silicon carbide.
[0014] In order to ensure the dressing efficiency, the binder of the CBN grinding wheel is quickly broken under the mechanical extrusion of the dresser and the dressing abrasive, exposing a new cutting edge. The particle size of the dressing abrasive is 1-3 particle sizes coarser than that of the CBN.
[0015] The grinding contact area of CBN grinding wheel is 10-100mm 2 , the thickness of the abrasive layer of the grinding wheel is 1-10mm.
[0016] The abrasive grain size of CBN grinding wheel is 80#~220#, and the grain size of dressing abrasive is 60#~600#.
[0017] The linear speed of the CBN grinding wheel is 20-40m / s, the linear speed of the dresser is 1-10m / s, and the feed speed of the workpiece is 0.2-0.6mm / min.
[0018] The present invention can well realize the online dressing of the ceramic bond CBN grinding wheel, has the advantages of high dressing efficiency, low consumption, good consistency of the blade height after dressing, and uniform dressing, and is a method capable of cyclic online grinding and dressing. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the principle of the present invention;
[0020] Figure 2 This is a schematic diagram of the trimming principle;
[0021] In the figure, 1 is a processing motor, 2 is a workpiece, 3 is a processing grinding wheel, 4 is a bidirectional motor, 5 is a dressed grinding wheel, 6 is a dresser, 7 is a dressing motor, 8 is a processing seat slide rail, 9 is a turntable, and 10 is a dressing seat slide rail. DETAILED DESCRIPTION
[0022] The present invention is described in detail below with reference to the accompanying drawings. The schematic diagram of the main process of the trimming method of the present invention is as follows: Figure 1As shown, the left side is a processing grinding wheel 3 that grinds the workpiece 2 (driven by a processing motor 1). When the grinding wheel needs to be dressed, the turntable 9 is rotated to switch the processing grinding wheel 3 and the dressed grinding wheel 5, and then the turntable 9 is fixed, so that the right side dressed grinding wheel 5 rotates to the left side to continue working, while the left side processing grinding wheel 3 rotates to the right side and is dressed by a dresser 6 driven by a dressing motor 7. During the dressing, a coolant and a dressing abrasive mixture are added; this is repeated and can be cyclically operated. The turntable can be rotated by mechanical methods, such as the method of meshing a gear driven by a motor with a rotating gear on the turntable shaft, the meshing of a chain driven by a motor with a rotating gear on the turntable shaft, and other commonly used methods; the processing motor is arranged on a processing seat, and the processing seat can move along the processing seat slide rail so that there is no interference when the turntable rotates. The movement of the processing seat can be achieved by a lead screw driven by a motor and a nut seat on the processing seat. When the lead screw and the motor connection end are fixed, the rotation of the lead screw can drive the processing seat to move back and forth; by the same token, the movement of the dressing seat on the dressing slide rail can be realized; the dressing fluid and the dressing abrasive are mixed in advance and added between the dresser and the dressing gear through a circulating water system.
[0023] Example 1
[0024] The online dressing method of the CBN grinding wheel of this embodiment adopts the following steps:
[0025] (1) First, the high-speed steel workpiece is ground with a ceramic bond CBN grinding wheel. The specifications of the CBN grinding wheel are shown in Table 1, and the specifications of the high-speed steel workpiece are shown in Table 2.
[0026] Table 1 Vitrified bond CBN grinding wheel
[0027] CBN particle size CBN concentration (vol%) Grinding contact area Grinding wheel abrasive layer thickness Number of grinding wheels 100 / 120 75 <![CDATA[35.6mm 2 ]]> 3mm 5
[0028] Table 2 Specifications of high speed steel
[0029] Steel Grade Hardness (HRC) Flexural strength(GPa) <![CDATA[Impact toughness (MJm 2 )]]> Grinding effective area W18Cr4V 65 3.8 0.3 20
[0030] (2) When the CBN grinding wheel is grinding the workpiece, the grinding wheel linear speed, workpiece linear speed, and workpiece feed speed are shown in Table 3. A total of 5 grinding cycles are performed, that is, 5 groups of vitrified bond CBN grinding wheels are used to grind the workpiece in a through-grinding manner.
[0031] Table 3 Grinding process parameters
[0032] Grinding wheel speed Workpiece linear speed Workpiece feed speed Grinding cycle times 25m / s 1m / s 0.3mm / min 5
[0033] The parameters of CBN grinding wheel when dressing CBN grinding wheel are shown in Table 1 and Table 3, and the specifications of dresser are shown in Table 4.
[0034] Table 4 Specifications of trimmer
[0035] Dresser diameter Dresser height Dresser Type Dresser line speed 20mm 30mm Bronze bond grinding wheel 2m / s
[0036] The specifications of the coolant and dressing abrasive mixed into the gap of the grinding wheel when dressing the CBN grinding wheel are shown in Table 5 below.
[0037] Table 5 Specifications of coolant and dressing abrasive
[0038] Coolant Type Abrasive particle size Abrasive Type BM-9 grinding fluid 80 Green Silicon Carbide
[0039] After the CBN grinding wheel is dressed, Table 6 shows the performance indicators of the CBN grinding wheel before and after grinding in this embodiment.
[0040] Table 6 Performance indicators of CBN grinding wheels before and after grinding
[0041] Serial number project CBN grinding wheel before grinding CBN grinding wheel after dressing 1 <![CDATA[1 cm under a 100x magnifying glass 2 Area abrasive grain exposure ratio]]> 98% 98% 2 Grinding wheel hardness before and after dressing (HRC) 75 76
[0042] Note: The grinding wheels before and after dressing refer to the unused CBN grinding wheels before grinding the workpiece and the CBN grinding wheels after dressing the workpiece.
[0043] From the above experimental data and test results, it can be seen that the present invention is a simple and effective method that can well realize the online dressing of ceramic bond CBN grinding wheels, has high dressing efficiency, low consumption, good consistency of blade height after dressing, uniform dressing, and can cycle online grinding and dressing.
[0044] To demonstrate the effective range of processing parameters, more experiments were conducted, such as Examples 2-4.
[0045] Example 2
[0046] The method of this embodiment is the same as that of embodiment 1, except that the following parameters are adjusted:
[0047] The dressing abrasive is made of corundum;
[0048] The grinding contact area of the CBN grinding wheel is 100mm 2 , the thickness of the abrasive layer of the grinding wheel is 6mm.
[0049] The abrasive grain size of the CBN grinding wheel is 80#, and the grain size of the dressing abrasive is 150#.
[0050] The linear speed of the CBN grinding wheel is 40 m / s, the linear speed of the dresser is 5 m / s, and the feed speed of the workpiece is 0.2 mm / min.
[0051] Example 3
[0052] The method of this embodiment is the same as that of embodiment 1, except that the following parameters are adjusted:
[0053] The dressing abrasive uses 50% of corundum and 50% of silicon carbide (volume ratio);
[0054] The grinding contact area of the CBN grinding wheel is 10mm 2 , the thickness of the abrasive layer of the grinding wheel is 1mm.
[0055] The abrasive grain size of the CBN grinding wheel is 220#, and the grain size of the dressing abrasive is 600#.
[0056] The linear speed of the CBN grinding wheel is 30 m / s, the linear speed of the dresser is 1 m / s, and the feed speed of the workpiece is 0.6 mm / min.
[0057] Example 4
[0058] The method of this embodiment is the same as that of embodiment 1, except that the following parameters are adjusted:
[0059] The dressing abrasive is made of silicon carbide;
[0060] The grinding contact area of the CBN grinding wheel is 50mm 2 , the thickness of the abrasive layer of the grinding wheel is 10mm.
[0061] The abrasive grain size of the CBN grinding wheel is 150#, and the grain size of the dressing abrasive is 400#.
[0062] The linear speed of the CBN grinding wheel is 20 m / s, the linear speed of the dresser is 10 m / s, and the feed speed of the workpiece is 0.4 mm / min.
Claims
1. A method for cyclic online grinding and dressing of a vitrified bond CBN grinding wheel, characterized in that: Through the external online measurement and data processing of the workpiece, the working state of the grinding wheel is judged, and the dressing curve of the grinding wheel is determined to determine the dressing time of the CBN grinding wheel; A bidirectional motor is arranged on the turntable, and CBN grinding wheels are fixed at both ends of the bidirectional motor. The CBN grinding wheel at one end processes the workpiece, and the CBN grinding wheel at the other end is dressed. When the processing grinding wheel needs to be dressed, the turntable is rotated to exchange the CBN grinding wheel used for processing with the CBN grinding wheel to be dressed, and the operation is repeated and cyclical. The grinding wheel dressing method is as follows: the coolant introduced into the grinding part is mixed with dressing abrasive, and the dressing abrasive can be well embedded in the binder of the CBN grinding wheel under the driving effect of the external radial grinding pressure and the coolant, so that the binder is broken and the ground CBN abrasive particles fall off, so as to realize the online dressing of the CBN grinding wheel; the hardness of the dressing abrasive should be lower than the hardness of the abrasive grains of the CBN grinding wheel, and the hardness of the dressing abrasive is higher than the hardness of the vitrified binder; this is conducive to breaking the binder of the CBN grinding wheel and avoiding physical and mechanical damage to the abrasive grains in the CBN grinding wheel.
2. The cyclic online grinding and dressing method of a vitrified bonded CBN grinding wheel according to claim 1, characterized in that: The material of the dressing abrasive can be selected from at least one of corundum and silicon carbide.
3. The cyclic online grinding and dressing method of a vitrified bonded CBN grinding wheel according to claim 2, characterized in that: Silicon carbide can be green silicon carbide.
4. The cyclic online grinding and dressing method of a vitrified bonded CBN grinding wheel according to claim 1, characterized in that: In order to ensure the dressing efficiency, the binder of the CBN grinding wheel is quickly broken under the mechanical extrusion of the dresser and the dressing abrasive, exposing a new cutting edge. The particle size of the dressing abrasive is 1-3 particle sizes coarser than that of the CBN.
5. The cyclic online grinding and dressing method of a vitrified bonded CBN grinding wheel according to claim 1, characterized in that: The grinding contact area of the CBN grinding wheel is 10-100mm2, and the thickness of the abrasive layer of the grinding wheel is 1-10mm.
6. The cyclic online grinding and dressing method of a vitrified bonded CBN grinding wheel according to claim 1, characterized in that: The abrasive grain size of CBN grinding wheel is 80#~220#, and the grain size of dressing abrasive is 60#~600#.
7. The cyclic online grinding and dressing method of a vitrified bonded CBN grinding wheel according to claim 1, characterized in that: The linear speed of the CBN grinding wheel is 20-40m / s, the linear speed of the dresser is 1-10m / s, and the feed speed of the workpiece is 0.2-0.6mm / min.
Citation Information
Patent Citations
Dynamic pressure releasing method of grinding liquid in grinding operation, grinding method using the releasing method, and grinding stone for use in the grinding method
CN101522372A
Method for dressing superhard abrasive grinding wheel by variable speed extruding and grinding of free abrasive grains under constraint of diamond surface
CN102229111A
Resin CBN (cubic boron nitride) end face grinding wheel and application
CN102814756A
Novel adjustable grinding machine
CN108515429A
Centerless grinding wheel online dressing method
CN108789156A