Optical fiber with high voltage resistance and low bending loss

By doping SiO2 and GeO2 in the core layer and sagging layer of the optical fiber, and doping Ge and F in the inner cladding, a step-type refractive index profile is formed, which solves the problem of excessive loss of ordinary optical fibers in deep sea environments and achieves It has stable data transmission performance under 11,000 meters of water and is suitable for deep-sea remote control and video signal transmission.

CN110609351BActive Publication Date: 2024-10-01ZHONGTIAN TECH ADVANCED MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201810615913.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-06-14
Publication Date
2024-10-01
Estimated Expiration
2038-06-14

AI Technical Summary

Technical Problem

Ordinary optical fibers cannot meet the data transmission needs under 11,000 meters of water due to excessive additional losses in deep-sea environments. The existing technology still has large losses at the ultimate diving depth of 7,000 meters and cannot meet the application needs of deeper waters.

Method used

An optical fiber with high voltage resistance and low bending loss is designed. By doping SiO2 and GeO2 in the core layer and sag layer, and doping Ge and F in the inner cladding and sag layer, a step refractive index profile is formed to reduce GeO2 Scattering loss caused by the fiber, and improving the withstand voltage performance of the optical fiber through appropriate F doping amount and sag layer width.

Benefits of technology

Under the pressure of 125MPa, the transmission loss at the 1550nm wavelength is no more than 0.001dB/km, and the attenuation at the 1310nm and 1550nm wavelengths is less than 0.5dB/km and 0.33dB/km, ensuring the transmission performance of the optical fiber in 11,000 meters deep water, suitable for remote control and large-capacity data transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110609351B_ABST
    Figure CN110609351B_ABST
Patent Text Reader

Abstract

The present invention provides an optical fiber with high pressure resistance and low bending loss, the optical fiber comprises a core layer, an inner cladding, a depression layer and an outer cladding, the core layer is doped with SiO2 and GeO2, the radius of the core layer is formed by extending the distance R1 outward from the center of the core layer, the refractive index of the core layer is n1, the width of the inner cladding is the distance R2-R1 extending outward from the edge R1 of the core layer, the profile of the inner cladding is formed by doping a small amount of Ge and F, the refractive index of the inner cladding is n2, the depression layer is deeply doped with F from the outer edge of the inner cladding to the outside, the width and refractive index of the depression layer are R3-R2 and n3 respectively, the thickness and refractive index of the outer cladding are Rc-R3 and nc respectively, and the refractive index profile of the optical fiber is a step-type distribution. The optical fiber provided by the present invention can still keep the optical fiber transmission performance unaffected in 11,000 meters of deep water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of optical fibers, and in particular to an optical fiber with high voltage resistance and low bending loss. Background Art

[0002] The ocean contains abundant water, oil, natural gas and mineral resources, which are of great significance to human survival and development. Optical cables can transmit data at high speed and long distances underwater. They have high transmission rate, small diameter and light weight. Ordinary optical fibers can basically meet the data transmission requirements in shallow sea areas, but with the increase of diving depth, ordinary optical fibers will eventually fail to transmit data due to the continuous increase of additional loss. At present, submarine signal transmission mainly selects suitable reinforcement and bonding materials on the outer layer of conventional G652 or G657 single-mode optical fiber, and uses the one-time molding process of reinforcing fiber and coating to improve the uniformity of surface radius, thereby reducing microbend loss. Its maximum diving depth is 7000 meters underwater, the maximum loss change at 1310nm wavelength is 0.015dB / km, and the maximum optical loss change at 1550nm is 0.059dB / km. Its loss is too large at a depth of 11,000 meters, causing data to be unable to be transmitted, and it cannot meet the application requirements at a depth of 11,000 meters. Summary of the invention

[0003] In view of this, it is necessary to provide an optical fiber that is resistant to high pressure and has low bending loss, wherein under high pressure conditions, the optical fiber loss is low and the transmission performance is not affected.

[0004] The present invention provides an optical fiber with high pressure resistance and low bending loss. The optical fiber comprises a core layer, an inner cladding, a depressed layer and an outer cladding. The core layer is doped with SiO2 and GeO2. The radius of the core layer is formed by a distance R1 extending outward from the center of the core layer. The refractive index of the core layer is n1. The width of the inner cladding is a distance R2-R1 extending outward from the edge R1 of the core layer. The cross section of the inner cladding is formed by doping a small amount of Ge and F. The refractive index of the inner cladding is n2. The depressed layer is deeply doped with F from the outer edge of the inner cladding to the outside. The width and refractive index of the depressed layer are R3-R2 and n3 respectively. The thickness and refractive index of the outer cladding are Rc-R3 and nc respectively. The refractive index profile of the optical fiber is a step-type distribution.

[0005] Furthermore, the core layer radius R1 is set between 2.5μm and 4μm, the width R2-R1 of the inner cladding is set between 2.5μm and 8μm, the width R3-R2 of the depressed layer is set between 3μm and 10μm, the radius Rc of the outer cladding is set between 40μm and 125μm, the refractive index difference n1-nc between the core layer and the outer cladding is between 0.01 and 0.016, the refractive index difference n2-nc between the inner cladding and the outer cladding is between -0.003 and 0.001, the refractive index difference n3-nc between the depressed layer and the outer cladding is between -0.003 and -0.01, and the refractive index difference between the core layer and the depressed layer satisfies n1-n3>0.016.

[0006] Furthermore, the outer cladding is a pure quartz glass layer, and the refractive index of the outer cladding is 1.4572.

[0007] Furthermore, the concentration range of GeO2 doped in the core layer is set between 14% and 19%, and the concentration range of GeO2 doped in the inner cladding layer is set between 0.8% and 2%.

[0008] Furthermore, the concentration range of the dopant F in the depressed layer is set between 0.5% and 1.5%.

[0009] Furthermore, the doping depth of the depressed layer is set at -0.0035 to -0.0053.

[0010] Furthermore, under a pressure of 125 MPa, a transmission loss variation of the optical fiber at a wavelength of 1550 nm is no greater than 0.001 dB / km.

[0011] Furthermore, the optical fiber has an attenuation of less than 0.5 dB / km at a wavelength of 1310 nm and an attenuation of less than 0.33 dB / km at a wavelength of 1550 nm.

[0012] Furthermore, the width of the depressed layer is greater than half of the mode field diameter of the optical fiber.

[0013] Furthermore, the deep F doping of the depressed layer is achieved by MCVD.

[0014] The high-voltage-resistant and low-bending-loss optical fiber of the present invention reduces the GeO2 doping amount in the core layer while the refractive index difference meets the design requirements by doping F in the depressed layer, thereby reducing the scattering loss caused by GeO2, and effectively increases the high-voltage resistance of the optical fiber by selecting a suitable F doping amount and a depressed width, and reduces the overall additional bending loss, ensuring that the optical fiber transmission performance is not affected in 11,000-meter deep water. The optical fiber is suitable for remote control of underwater navigation equipment, operation monitoring, and remote transmission of large-capacity data such as video signals, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 Schematic diagram of the cross section and refractive index profile of the optical fiber in one embodiment of the present invention.

[0016] Figure 2 This is a data parameter diagram of the optical fiber cross-sectional structure in one embodiment of the present invention.

[0017] Figure 3 This is a diagram of the withstand voltage test data of the optical fiber in one embodiment of the present invention.

[0018] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] It should be noted that when a component is considered to be “disposed on” another component, it may be directly disposed on the other component or there may be a central component at the same time.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "or / and" used herein includes any and all combinations of one or more of the related listed items.

[0022] See also Figure 1 , Figure 1 The cross-section and refractive index profile of the optical fiber in one embodiment of the present invention is a schematic diagram, wherein the optical fiber is used for signal transmission in 11,000-meter-deep water, and the optical fiber includes a core layer, an inner cladding layer, a depression layer, and an outer cladding layer sequentially coated from the inside to the outside. In this embodiment, the optical fiber is a single-mode optical fiber.

[0023] The radius of the core layer is formed by the distance R1 extending outward from the center of the core layer, the refractive index of the core layer is n1, the core layer radius R1 is set between 2.5μm and 4μm, and the refractive index difference Δ1 between the core layer and the outer cladding is set between 0.01 and 0.016. In this embodiment, the core layer is doped with SiO2 and GeO2, and the concentration range of the core layer doped with GeO2 is set between 14% and 19%. Reducing the amount of GeO2 doped in the core layer can effectively reduce the scattering loss caused by GeO2. In other embodiments, the core layer can also be doped with a small amount of F.

[0024] The inner cladding is coated on the core layer, and the distance R2 extending outward from the center of the core layer is the width of the core layer and the inner cladding, that is, the width of the inner cladding is R2-R1, the refractive index of the inner cladding is n2, the width R2-R1 of the inner cladding is set between 2.5μm and 8μm, and the refractive index difference Δ2 between the inner cladding and the outer cladding is set between -0.003 and 0.001. In this embodiment, the cross section of the inner cladding is formed by doping a small amount of Ge and F, and the concentration range of the inner cladding doped with GeO2 is set between 0.8% and 2%.

[0025] The depressed layer is coated on the inner cladding, and the depressed layer is deeply doped with F from the outer edge of the inner cladding to the outside. The doping with F is used to reduce the refractive index. The optical fiber bending loss gradually decreases with the increase of the width and depth of the depressed layer. The doping depth of the depressed layer is set at about -0.005, which can well improve the optical fiber bending loss performance. In this embodiment, the doping depth of the depressed layer is set at -0.0035 to -0.0053, and the concentration range of the dopant F in the depressed layer is set between 0.5% and 1.5%. The doping of F in the depressed layer is achieved by MCVD process. In other embodiments, the doping of F in the depressed layer can also be achieved by PCVD.

[0026] The distance R3 extending outward from the center of the core layer is the total width of the core layer, the inner cladding layer and the depressed layer, that is, the width of the depressed layer is R3-R2, and the width R3-R2 of the depressed layer is set between 3μm and 10μm. Due to the influence of the width of the depressed layer on the cut-off wavelength and bending loss performance, the width of the depressed layer is set to be greater than half of the mode field diameter of the optical fiber, and the refractive index of the depressed layer is n3, and the refractive index difference Δ3 between the depressed layer and the outer cladding is set between -0.003 and -0.01. In this embodiment, the refractive index difference between the core layer and the depressed layer satisfies n1-n3>0.016.

[0027] The radius Rc of the outer cladding is set between 40 μm and 125 μm, and the refractive index of the outer cladding is nc. In this embodiment, the outer cladding is a pure quartz glass layer, so the refractive index nc of the outer cladding is 1.4572.

[0028] The refractive index profile of the optical fiber is a step-type distribution. The optical fiber attenuation is less than 0.5dB / km at a wavelength of 1310nm and less than 0.33dB / km at a wavelength of 1550nm. In order to improve the bending resistance of the optical fiber, the optical fiber cutoff wavelength should be between 1450nm and 1530nm.

[0029] The present invention will be further described below in conjunction with specific embodiments.

[0030] Example 1

[0031] The core layer radius R1 is 2.95μm, the refractive index difference Δ1 between the core layer and the outer cladding is 0.0152, the inner cladding thickness R2-R1 is 5.05μm, the refractive index difference Δ2 between the inner cladding and the outer cladding is 0.001, the F-doping depth of the depressed layer is -0.0035, the width R3-R2 of the depressed layer is 6.1μm, the radius Rc of the outer cladding is 62.5μm, the refractive index difference n1-n3 between the core layer and the depressed layer is 0.0187, the mode field diameter of the optical fiber under this design is 6.2μm, and the cut-off wavelength of the optical fiber is 1462nm.

[0032] Example 2

[0033] The core layer radius R1 is 3.25μm, the refractive index difference Δ1 between the core layer and the outer cladding is 0.013, the inner cladding thickness R2-R1 is 4.95μm, the refractive index difference Δ2 between the inner cladding and the outer cladding is -0.0007, the F-doping depth of the depressed layer is -0.0053, the width R3-R2 of the depressed layer is 5.6μm, the radius Rc of the outer cladding is 62.5μm, the refractive index difference n1-n3 between the core layer and the depressed layer is 0.0183, the mode field diameter of the optical fiber under this design is 6.6μm, and the cut-off wavelength of the optical fiber is 1479nm.

[0034] Example 3

[0035] The core layer radius R1 is 3.65μm, the refractive index difference Δ1 between the core layer and the outer cladding is 0.0116, the inner cladding thickness R2-R1 is 4.9μm, the refractive index difference Δ2 between the inner cladding and the outer cladding is -0.0007, the F-doping depth of the depressed layer is -0.0053, the width R3-R2 of the depressed layer is 5.9μm, the radius Rc of the outer cladding is 62.5μm, the refractive index difference n1-n3 between the core layer and the depressed layer is 0.0183, the mode field diameter of the optical fiber under this design is 7.4μm, and the cut-off wavelength of the optical fiber is 1484nm.

[0036] See also Figure 2 and Figure 3 , Figure 2 It is a data parameter diagram of the optical fiber cross-sectional structure described in Example 2, wherein the horizontal axis is the radius and the vertical axis is the refractive index. Figure 3 The pressure test results of the optical fiber described in Example 2 are shown under gradually increasing pressure conditions of 0-125MPa. It can be seen that the loss change value of the optical fiber designed in Example 2 at a wavelength of 1550nm under a pressure of 125MPa is 0.001dB / km, which can meet the data transmission requirements at 110MPa in the deep sea.

[0037] The high-voltage-resistant and low-bending-loss optical fiber of the present invention reduces the GeO2 doping amount in the core layer while the refractive index difference meets the design requirements by doping F in the depressed layer, thereby reducing the scattering loss caused by GeO2, and effectively increases the high-voltage resistance of the optical fiber by selecting a suitable F doping amount and a depressed width, and reduces the overall additional bending loss, ensuring that the optical fiber transmission performance is not affected in 11,000-meter deep water. The optical fiber is suitable for remote control of underwater navigation equipment, operation monitoring, and remote transmission of large-capacity data such as video signals, and has broad application prospects.

[0038] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit and scope of the present invention, appropriate changes and modifications to the above embodiments are within the scope of protection claimed by the present invention.

Claims

1. An optical fiber with high voltage resistance and low bending loss, characterized in that: The optical fiber comprises a core layer, an inner cladding, a depression layer and an outer cladding, the core layer is doped with SiO2 and GeO2, the radius of the core layer is formed by a distance R1 extending outward from the center of the core layer, the refractive index of the core layer is n1, the width of the inner cladding is a distance R2-R1 extending outward from the edge R1 of the core layer, the profile of the inner cladding is formed by doping a small amount of Ge and F, the refractive index of the inner cladding is n2, the depression layer is deeply doped with F from the outer edge of the inner cladding outward, the width and refractive index of the depression layer are R3-R2 and n3 respectively, the thickness and refractive index of the outer cladding are Rc-R3 and nc respectively, and the refractive index profile of the optical fiber is a step-type distribution; the core layer radius R1 is set between 2.5μm and 4μm, the width R2-R1 of the inner cladding is set between 2.5μm and 8μm, the width R3-R2 of the depression layer is set between 2.5μm and 8μm, and the width R3-R2 of the depression layer is set between 2.5μm and 8μm. The refractive index difference between the core layer and the outer cladding is n1-nc, the refractive index difference between the inner cladding and the outer cladding is n2-nc, the refractive index difference between the depression layer and the outer cladding is n3-nc, the refractive index difference between the core layer and the depression layer satisfies n1-n3>0.016; the concentration range of GeO2 doped in the core layer is set between 14% and 19%, the concentration range of GeO2 doped in the inner cladding is set between 0.8% and 2%; the concentration range of the dopant F in the depression layer is set between 0.5% and 1.5%; the width of the depression layer is set to be greater than half of the mode field diameter of the optical fiber.

2. The optical fiber with high voltage resistance and low bending loss as claimed in claim 1, characterized in that: The outer cladding is a pure quartz glass layer, and the refractive index of the outer cladding is 1.4572.

3. The optical fiber with high voltage resistance and low bending loss as claimed in claim 1, characterized in that: The doping depth of the depressed layer is set at -0.0035 to -0.0053.

4. The optical fiber with high voltage resistance and low bending loss as claimed in claim 1, characterized in that: The transmission loss variation value of the optical fiber at a wavelength of 1550nm is no more than 0.001dB / km under a pressure of 125MPa.

5. The optical fiber with high voltage resistance and low bending loss as claimed in claim 1, characterized in that: The optical fiber has an attenuation of less than 0.5 dB / km at a wavelength of 1310 nm and an attenuation of less than 0.33 dB / km at a wavelength of 1550 nm.

6. The optical fiber with high voltage resistance and low bending loss as claimed in claim 1, characterized in that: The deep F doping of the depressed layer is achieved by MCVD.