A two-dimensional organic-inorganic heterojunction encapsulated by boron nitride and preparation method thereof
By using boron nitride as the packaging layer and the combination of hole-laden gold electrode and liquid metal glue, the problems of contamination and insufficient adhesion during the two-dimensional organic-inorganic heterocarrier transfer and packaging process in the prior art are solved, and high Quality and high efficiency heterocarrier transfer and packaging improves electron mobility and transfer success rate.
Patent Information
- Application Number
- CN201911071005.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-11-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-11-05
AI Technical Summary
During the production, transfer and packaging of existing two-dimensional organic-inorganic van der Waals heterojunctions, wet transfer introduces chemical additives to contaminate the interface, resulting in a decline in material quality, while polydimethylsilic oxygen used in dry transfer is used. The adhesion of the alkane substrate is weak and the transfer success rate is not high.
Boron nitride is used as the encapsulation layer to epitaxially grow organic films by chemical vapor deposition method, and the hole-laden gold electrode and liquid metal glue are used to improve adhesion, achieving rapid and accurate heterocarrier transfer and packaging.
The quality and transfer success rate of two-dimensional nanomaterials are improved, electron mobility is increased, and high efficiency is maintained in the atmospheric environment, carrier mobility is improved, and the transfer process is simplified and accurate.
Smart Images

Figure CN110676384B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of two-dimensional semiconductor materials, and in particular to a two-dimensional organic-inorganic heterojunction encapsulated by boron nitride and a preparation method thereof. Background Art
[0002] As a new type of material, two-dimensional semiconductor materials have attracted widespread attention since the discovery of single-layer graphene in 2004. It is a new type of material with the advantages of high mechanical strength, high thermal conductivity, high mobility, ultra-thin transparency, and flexible rollability. Its excellent optical and electrical properties have made breakthroughs in optoelectronics, biology, storage, flexibility, integrated circuits and other fields.
[0003] There are two main methods for preparing heterojunctions: chemical epitaxial growth and physical vapor deposition, of which the more famous ones are molecular beam epitaxy (MBE) and metal organic chemical vapor deposition (MOCVD). The high-quality heterostructures prepared by these two methods have made important contributions to the construction of advanced functional devices such as transistors with high electron mobility, LEDs and quantum cascade lasers.
[0004] However, the heterojunctions constructed by these two types of technologies rely on one-to-one chemical bonding, which requires extremely high lattice matching of the two materials. For chemical epitaxial growth, lattice mismatch easily leads to the formation of polycrystalline, and the interface is greatly affected by strain; for physical vapor deposition, the requirements for material type and lattice matching are relatively flexible, but the deposited materials are mostly amorphous or polycrystalline, and the interface is easily disturbed by defects or chemical disorders.
[0005] Van der Waals heterojunctions are physically assembled together through relatively weak van der Waals interactions, do not rely on chemical bonds, and are not limited by the lattice matching of materials, bringing new hope to the electronic and optoelectronic device industries. In principle, if there are no special requirements for lattice similarity and processing compatibility, this van der Waals heterojunction integration strategy is applicable to any material, especially for the flexible integration of materials with different crystal structures, different electronic properties, different sizes and dimensions.
[0006] The covalently bonded atomic layers in two-dimensional layered materials are weakly bound to each other through van der Waals interactions, which provides considerable flexibility for separating, mixing and matching individual atomic layers without being restricted by lattice and processing compatibility. Therefore, it can open up broad possibilities for almost arbitrary combinations of multiple materials and integration of different properties at the atomic scale, making possible entirely new opportunities that are out of reach of existing materials.
[0007] At present, dry transfer or wet transfer is mainly used in the production, transfer and packaging of two-dimensional organic-inorganic van der Waals heterojunctions. Among them, the wet transfer process requires the introduction of chemical additives to assist the dissociation of two-dimensional nanomaterials, detachment from the original substrate surface, and removal of the transfer medium, which will introduce other chemical reagents to contaminate the interface, resulting in a decrease in the quality of the two-dimensional nanomaterials. Dry transfer requires the use of a polydimethylsiloxane (PDMS) substrate as a transfer medium, which introduces almost no contamination, so the quality of the samples obtained is generally higher than that of wet transfer, but the disadvantage is that the adhesion of (PDMS) as a substrate is weak, and the transfer success rate is not high. Summary of the invention
[0008] Purpose of the invention: To provide a boron nitride encapsulated two-dimensional organic-inorganic heterojunction and a preparation method thereof, so as to solve the problems involved in the above-mentioned background technology.
[0009] Technical solution: A two-dimensional organic-inorganic heterojunction encapsulated by boron nitride, including four parts: a substrate, a bottom encapsulation layer, a two-dimensional nanolayer and a top encapsulation layer.
[0010] Among them, the substrate is made of silicon wafer; the bottom encapsulation layer is made of two-dimensional boron nitride and is arranged on the substrate; the two-dimensional nanolayer is a layered heterojunction structure formed by at least two layers of two-dimensional organic materials and / or two-dimensional inorganic materials, and is arranged on the bottom encapsulation layer; the top encapsulation layer is made of two-dimensional boron nitride and is arranged on the other side of the two-dimensional nanolayer.
[0011] The method for preparing the two-dimensional organic-inorganic heterojunction based on the boron nitride encapsulation comprises the following steps:
[0012] S1, transferring the two-dimensional boron nitride to a silicon wafer substrate as a bottom encapsulation layer for encapsulation, and epitaxially growing an organic thin film on the boron nitride of the bottom encapsulation layer by chemical vapor deposition;
[0013] S2, transferring the two-dimensional boron nitride of the top encapsulation layer to the surface of the silicon wafer, and covering the boron nitride with a gold electrode with holes, the exposed hole area of the gold electrode is placed on the two-dimensional layered boron nitride, and the area of the two-dimensional boron nitride should be larger than the area of the square hole, and high-temperature heating is performed;
[0014] S3, using a fine needle to bring up the two-dimensional boron nitride of the gold electrode and the top encapsulation layer, and placing the two-dimensional boron nitride on the two-dimensional inorganic material to be transferred;
[0015] S4. Under an optical microscope, use a fine needle to pick up the gold electrode, the two-dimensional boron nitride of the top encapsulation layer, and the two-dimensional inorganic material, and place them on the boron nitride of the bottom encapsulation layer with the organic thin film grown thereon. Align the two-dimensional inorganic material and the two-dimensional organic layer through the square hole on the gold electrode, and place the whole on the boron nitride of the bottom encapsulation layer with the organic thin film grown thereon.
[0016] S5. Use a fine needle to lift off the gold electrode on the top encapsulated two-dimensional boron nitride.
[0017] S6. Finally, the prepared boron nitride encapsulated heterojunction is placed in a vacuum device to make the two-dimensional organic material and / or the two-dimensional inorganic material fit tightly.
[0018] As a preferred embodiment, the two-dimensional boron nitride is prepared by mechanical exfoliation or chemical vapor deposition.
[0019] As a preferred solution, the organic film comprises one or more organic semiconductor materials selected from the group consisting of semiconductor perylenetetracarboxylic dianhydride, semiconductor perylene diimide, semiconductor dioctylbenzothiophene-benzothiophene, and N,N'-dimethyldicarboximide.
[0020] As a preferred solution, the gold electrode is made by electron beam exposure technology, and a hollow small hole is arranged on the gold electrode. A hollow square small hole with a side length of 20 um is arranged on the gold electrode.
[0021] As a preferred solution, the gold electrode is covered on the boron nitride and then heated in a vacuum at 200-260°C.
[0022] As a preferred embodiment, the two-dimensional material to be transferred is obtained by mechanical exfoliation to obtain a two-dimensional inorganic material on silicon oxide.
[0023] As a preferred solution, the tip of the fine needle is dipped in a metal glue that is liquid at room temperature, which serves as glue for bonding the gold electrode.
[0024] Beneficial effects: The present invention relates to a boron nitride encapsulated two-dimensional organic-inorganic heterojunction and a preparation method thereof. By using boron nitride instead of a traditional glass film as an encapsulation layer, it can not only play a good encapsulation role, but also isolate the influence of external water and oxygen on the two-dimensional material, and can increase the electron mobility. By combining the liquid metal glue with the gold electrode with holes, the adhesion between the liquid metal glue and the two-dimensional material is improved, and the transfer success rate and accuracy are improved. Moreover, the gold electrode with holes is used as a support layer, which is convenient for later removal and can achieve rapid transfer and precise alignment. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic structural diagram of the boron nitride encapsulated organic-inorganic van der Waals heterojunction of the present invention.
[0026] Figure 2 It is a schematic diagram of placing a gold electrode on the top packaging layer as a supporting layer top packaging in the present invention.
[0027] Figure 3It is a schematic diagram of transferring the bottom packaging layer covered with gold electrodes onto a two-dimensional inorganic material according to the present invention.
[0028] Figure 4 It is a schematic diagram of transferring a two-dimensional inorganic material layer and a top encapsulation layer onto a two-dimensional organic material and a bottom encapsulation layer according to the present invention.
[0029] The reference numerals are: substrate 1 , bottom encapsulation layer 2 , two-dimensional organic material 3 , two-dimensional inorganic material 4 , top encapsulation layer 5 , gold electrode 6 , fine needle 7 . DETAILED DESCRIPTION
[0030] In the following description, a large number of specific details are provided to provide a more thorough understanding of the present invention. However, it is apparent to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features well known in the art are not described.
[0031] As attached Figure 1 As shown, a two-dimensional organic-inorganic heterojunction encapsulated by boron nitride includes four parts: a substrate 1, a bottom encapsulation layer 2, a two-dimensional nanolayer and a top encapsulation layer 5. Among them, the substrate 1 is made of a silicon wafer; the bottom encapsulation layer 2 is made of a two-dimensional boron nitride and is arranged on the substrate 1; the two-dimensional nanolayer is a layered heterojunction structure formed by at least two layers of two-dimensional organic materials 3 and / or two-dimensional inorganic materials 4, and is arranged on the bottom encapsulation layer 2; the top encapsulation layer 5 is made of a two-dimensional boron nitride and is arranged on the other side of the two-dimensional nanolayer. More specifically, the thickness of the bottom encapsulation layer and the bottom encapsulation layer is 40-50nm, and the thickness of the two-dimensional nanolayer is 4-10nm; wherein the thickness ratio between the two-dimensional organic material and the two-dimensional inorganic material is 1: (1-2). The two-dimensional nanolayer is connected to the top encapsulation layer and the top encapsulation layer by liquid metal glue, preferably indium gallium alloy as the glue for bonding the gold electrode 6, and its thickness is 10-20nm, which has a stronger bonding force than the bonding force between atomic layers.
[0032] Since hexagonal boron nitride is an insulating layered two-dimensional material, it has a crystal structure that is highly similar to graphene. Therefore, in the process of preparing a two-dimensional organic-inorganic heterojunction, hexagonal boron nitride is directly used for encapsulation to further enhance the optical and electrical properties of the heterojunction. This structure gives it extremely high high temperature stability and a smooth surface at the atomic level. In addition, there are very few dangling bonds and charge traps on the surface of hexagonal boron nitride, providing a uniform dielectric environment for two-dimensional materials. It effectively reduces the scattering or capture of photogenerated carriers by impurity defects, so that the material has an ultra-long carrier migration distance, a long carrier lifetime, and a high carrier mobility, thereby improving the optical and electrical properties of the material. Therefore, compared with the encapsulation process of traditional glass film, the above-mentioned hexagonal boron nitride not only has a good encapsulation effect, but also can isolate the influence of external water and oxygen on two-dimensional materials and increase electron mobility. As a preferred embodiment, two-dimensional boron nitride is prepared by mechanical stripping or chemical vapor deposition.
[0033] Among them, the two-dimensional nanolayer is a layered heterojunction structure formed by at least two layers of two-dimensional organic material 3 and / or two-dimensional inorganic material 4. It is a functional semiconductor material that determines the use of the semiconductor sensor. It can be but is limited to photosensitive materials, temperature-sensitive materials, and pressure-sensitive materials for solar cells. The above-mentioned two-dimensional organic materials 3 and two-dimensional inorganic materials 4 are all known materials, so no specific restrictions are made here. In the specific implementation process, the two-dimensional organic material 3 includes but is not limited to organic semiconductor materials such as semiconductor perylene tetracarboxylic dianhydride (PTCDA), semiconductor perylene diimide (PTCDI), semiconductor dioctylbenzothiophene and benzothiophene (C8-BTBT), N, N'-dimethyl dicarboximide (MEPTCDI), etc. Inorganic materials include, but are not limited to, inorganic semiconductor materials such as cadmium sulfide, tin sulfide, silver sulfide, antimony sulfide, lead sulfide, zinc sulfide, indium sulfide, cadmium selenide, tin selenide, silver selenide, antimony selenide, lead selenide, zinc selenide, and indium selenide, and can also be inorganic semiconductor materials composed of sulfides or selenides of metal elements in the third main group, the fourth main group, and the fifth main group. Among them, taking the photosensitive material for solar cells as an example, C8-BTBT of the two-dimensional organic material 3 is preferably used as a hole transport layer to collect electron-hole pairs and realize the transmission of electrons, and two-dimensional silver selenide is preferably used as a photosensitive material to realize the absorption of light energy.
[0034] The present invention will be further described below in conjunction with embodiments. The examples of the embodiments are intended to explain the present invention and should not be construed as limiting the present invention.
[0035] Example 1
[0036] A method for preparing a two-dimensional organic-inorganic heterojunction based on the above-mentioned boron nitride encapsulation comprises the following process steps:
[0037] S1, transfer the two-dimensional boron nitride to the silicon wafer substrate 1 for bottom packaging. The method of mechanical stripping and transfer of the two-dimensional boron nitride is as follows: place the hexagonal boron nitride of the block material on the sticky side of the tape, use other tapes to repeatedly tear it apart, so that the boron nitride is thinned to a predetermined thickness, and finally stick the tape with the hexagonal boron nitride to the silicon dioxide surface, press it lightly, and then remove it, so as to obtain the two-dimensional boron nitride on the silicon wafer.
[0038] S2. Epitaxially grow an organic film on boron nitride using chemical vapor deposition (CVD). The two-dimensional boron nitride used as the bottom package is placed in a CVD tube furnace for growth, so that a layer of organic film grows evenly on the two-dimensional boron nitride. The CVD growth method is as follows: 1. Place the growth source of the two-dimensional organic material 3 (C8-BTBT is selected as the growth source in this embodiment) and the hexagonal boron nitride matrix in a CVD tube furnace, respectively, and place them at intervals; 2. Pass argon gas and heat at 200-260°C for 3h; 3. Cool naturally to obtain a layered organic material grown on boron nitride.
[0039] S3, transfer the two-dimensional boron nitride of the top encapsulation layer to the surface of the silicon wafer, and cover the boron nitride of the top encapsulation layer 5 with a gold electrode 6 with a hole. With the help of an optical microscope, cover the boron nitride as the top encapsulation with a gold electrode 6 with a hole (and the area of the two-dimensional boron nitride should be larger than the area of the square hole, and high temperature heating is performed), and the gold electrode 6 is covered with the boron nitride and heated at 200-260°C in a vacuum for 45 minutes. The specific steps are as follows Figure 2 As shown, a gold electrode 6 with a hole is adhered by a metal needle, wherein the gold electrode 6 should have a hollow small hole, the length and width of the small hole are 20um, and it is made by electron beam exposure method. The specific method of the electron beam exposure method is: a layer of bottom electron beam resist is coated on the two-dimensional boron nitride, and a metal layer, preferably gold, is covered on the bottom electron beam resist. Since gold is soft, it is convenient for further processing later; and a top layer of electron beam resist is coated on the non-etched area of the metal layer; the temperature tolerance of the electron beam resist is greater than the electron beam exposure temperature, and then electron beam exposure is performed to form a gold electrode 6 with a hole. Or it can be made by electron beam exposure method on other processing materials and then transferred to two-dimensional boron nitride.
[0040] S4. With the help of an optical microscope, use a fine needle 7 to pick up the gold electrode 6 covered with holes and the two-dimensional boron nitride, and place the material on the two-dimensional inorganic material 4 to be transferred; wherein the tip of the fine needle 7 is dipped in a metal glue that is liquid at room temperature as the glue for bonding the gold electrode 6. In this embodiment, indium gallium alloy is selected as the glue for bonding the gold electrode 6, and silver selenide is selected as the two-dimensional inorganic material 4. The specific steps are as follows Figure 2As shown, the two-dimensional organic material 3 to be transferred is subjected to mechanical exfoliation to obtain the two-dimensional inorganic material 4 on silicon oxide. The specific mechanical exfoliation process is the same as step S1.
[0041] S5, as above, use a fine needle 7 to bring up the gold electrode 6, the boron nitride of the top encapsulation layer and the two-dimensional inorganic material 4, align the two-dimensional inorganic material and the two-dimensional organic layer through the square hole on the gold electrode, and place the whole on the boron nitride of the bottom encapsulation layer with the organic film grown. The specific steps are as follows Figure 3 shown.
[0042] S6. Use a fine needle 7 under an optical microscope to lift off the gold electrode 6 with a hole; finally, place the prepared boron nitride encapsulated heterojunction in a vacuum device to make the two-dimensional organic material 3 and / or the two-dimensional inorganic material 4 fit tightly.
[0043] When boron nitride is used to encapsulate the organic-inorganic van der Waals heterojunction, the cell conversion efficiency of the organic-inorganic van der Waals heterojunction is 1.06% before encapsulation and 1.18% after encapsulation. After the encapsulated cell is placed in the atmosphere for 1000 hours, the efficiency is 1.09%. And the carrier mobility of the organic-inorganic van der Waals heterojunction can be as high as 53.14cm 2 / (V•s). On the other hand, the average time consumed in the transfer process is about 2 minutes.
[0044] Example 2
[0045] A method for preparing a two-dimensional organic-inorganic heterojunction based on the above-mentioned boron nitride encapsulation comprises the following process steps:
[0046] S1, transferring the two-dimensional layered material of the glass film onto the silicon wafer substrate 1 for bottom encapsulation, wherein the peeling and transfer methods are the same as those in Example 1.
[0047] S2, epitaxially grow an organic thin film on the glass thin film by chemical vapor deposition (CVD), and place the glass thin film as the bottom package in a CVD tube furnace for growth, so that a layer of organic thin film grows uniformly on the glass thin film. The CVD growth method is the same as in Example 1.
[0048] S3, the glass film of the top encapsulation layer 5 is covered with a gold electrode 6 with a hole. With the help of an optical microscope, the glass film as the top encapsulation is covered with a gold electrode 6 with a hole, and the gold electrode 6 is heated at 200-260° C. for 45 minutes in a vacuum after being covered with the glass film. For specific steps, refer to Example 1.
[0049] S4. With the assistance of an optical microscope, a fine needle 7 (the tip of the fine needle 7 is dipped in a metal glue that is liquid at room temperature, which is used as glue for bonding the gold electrode 6. Indium gallium alloy is selected in this embodiment) is used to pick up the gold electrode 6 and the glass film material covered with holes, and the material is placed on the two-dimensional inorganic material 4 to be transferred. The specific steps are as follows: Figure 2 As shown. The two-dimensional organic material 3 to be transferred is subjected to mechanical exfoliation to obtain the two-dimensional inorganic material 4 on silicon oxide. The specific process is the same as step S1 in Example 1.
[0050] S5, same as above, use a fine needle 7 to bring up the gold electrode 6, the glass film and the two-dimensional inorganic material 4, align the two-dimensional inorganic material and the two-dimensional organic layer through the square hole on the gold electrode, and place the whole on the glass film with the organic film grown; the specific steps are as follows Figure 3 shown.
[0051] S6. Use a fine needle 7 under an optical microscope to lift off the gold electrode 6 with a hole; finally, place the prepared glass film-encapsulated heterojunction in a vacuum device to make the two-dimensional organic material 3 and / or the two-dimensional inorganic material 4 fit tightly.
[0052] When the organic-inorganic van der Waals heterojunction is encapsulated with a glass film, the conversion efficiency of the organic-inorganic van der Waals heterojunction is 1.06% before encapsulation and 0.88% after encapsulation. After the encapsulated battery is placed in the atmosphere for 1000 hours, the efficiency is 0.74%. And the carrier mobility of the organic-inorganic van der Waals heterojunction can be as high as 42.25cm 2 / (V•s). On the other hand, the average time consumed in the transfer process is about 2 minutes.
[0053] Example 3
[0054] A method for preparing a two-dimensional organic-inorganic heterojunction based on the above-mentioned boron nitride encapsulation comprises the following process steps:
[0055] S1, transferring the two-dimensional layered material of the glass film to the surface of the silicon wafer as the substrate 1 and the bottom package. The peeling and transfer methods are referred to in Example 1.
[0056] S2. Spin-coat a layer of polymethyl dimethacrylate as a release agent evenly on the silicon wafer substrate 1 at high speed, bake at 250° C. for 5 min to remove the solvent, use a capillary pipette to take up the glass film material, and place the glass film on the silicon wafer substrate 1.
[0057] S3, epitaxially growing an organic thin film on the glass film by chemical vapor deposition (CVD), placing the glass film as the bottom package in a CVD tube furnace for growth, so that a layer of organic thin film is uniformly grown on the glass film. The CVD growth method is the same as in Example 1.
[0058] S4. Similarly, with the assistance of an optical microscope, a capillary pipette is used to pick up the two-dimensional inorganic material 4 to be transferred and place the glass film on the organic film.
[0059] S5. Finally, the prepared glass film-encapsulated heterojunction is placed in a vacuum device to make the two-dimensional organic material 3 and / or the two-dimensional inorganic material 4 fit tightly.
[0060] When the organic-inorganic van der Waals heterojunction is encapsulated with a glass film, the conversion efficiency of the organic-inorganic van der Waals heterojunction is 1.06% before encapsulation and 0.90% after encapsulation. After the encapsulated battery is placed in the atmosphere for 1000 hours, the efficiency is 0.74%. And the carrier mobility of the organic-inorganic van der Waals heterojunction can be as high as 40.98cm 2 / (V•s). On the other hand, the average time consumed in the transfer process is about 10 min, which is much longer than the time consumed when using gold electrodes for transfer.
[0061] Compared with Examples 1 to 3, boron nitride is used instead of the traditional glass film as the encapsulation layer, which not only plays a good encapsulation role, but also isolates the influence of external water and oxygen on the two-dimensional material, and can increase the electron mobility. In addition, since the gold electrode is about 100nm thick, soft and has a certain mechanical strength, it is an excellent supporting material. Thin two-dimensional boron nitride is transparent when there is no substrate, and the square hole can be used to clearly see what needs to be transferred to the target substrate. And the thin two-dimensional boron nitride as a supporting layer has less refraction of light, which is more convenient for alignment. By combining the liquid metal glue with the gold electrode 6 with holes, the adhesion between it and the two-dimensional material is increased, thereby greatly improving the transfer success rate. The force between the gold electrode and the two-dimensional material is relatively weak, and it is easier to separate without loss, and there is no residue, which is convenient for later removal.
[0062] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A two-dimensional organic-inorganic heterojunction encapsulated by boron nitride, characterized in that: include: A substrate, the material of which is a silicon wafer; A bottom encapsulation layer, made of two-dimensional boron nitride, is disposed on the substrate, wherein the two-dimensional boron nitride is layered hexagonal boron nitride; A two-dimensional nanolayer, a layered heterojunction structure formed by at least two layers of two-dimensional organic materials and / or two-dimensional inorganic materials, and disposed on the bottom encapsulation layer; A top encapsulation layer, made of two-dimensional boron nitride, is disposed on the other side of the two-dimensional nanolayer; The preparation method of a two-dimensional organic-inorganic heterojunction based on boron nitride encapsulation specifically includes: S1, transferring the two-dimensional boron nitride to a silicon wafer substrate as a bottom encapsulation layer for encapsulation, and epitaxially growing an organic thin film on the boron nitride of the bottom encapsulation layer by chemical vapor deposition; S2, transferring the two-dimensional boron nitride of the top encapsulation layer to the surface of the silicon wafer, and covering the boron nitride with a gold electrode with holes, the exposed hole area of the gold electrode is placed on the two-dimensional layered boron nitride, and the area of the two-dimensional boron nitride should be larger than the area of the square hole, and high-temperature heating is performed; S3, using a fine needle to bring up the two-dimensional boron nitride of the gold electrode and the top encapsulation layer, and placing the two-dimensional boron nitride on the two-dimensional inorganic material to be transferred; S4. Under an optical microscope, use a fine needle to pick up the gold electrode, the two-dimensional boron nitride of the top encapsulation layer, and the two-dimensional inorganic material, and place them on the boron nitride of the bottom encapsulation layer with the organic thin film grown thereon. Align the two-dimensional inorganic material and the two-dimensional organic layer through the square hole on the gold electrode, and place the whole on the boron nitride of the bottom encapsulation layer with the organic thin film grown thereon. S5. Use a fine needle to remove the gold electrode on the top encapsulated two-dimensional boron nitride; S6. Finally, the prepared boron nitride encapsulated heterojunction is placed in a vacuum device to make the two-dimensional organic material and / or the two-dimensional inorganic material fit tightly.
2. The boron nitride encapsulated two-dimensional organic-inorganic heterojunction according to claim 1, characterized in that: The two-dimensional boron nitride is prepared by a mechanical exfoliation method or a chemical vapor deposition method.
3. The boron nitride encapsulated two-dimensional organic-inorganic heterojunction according to claim 1, characterized in that: The organic film comprises one or more organic semiconductor materials selected from the group consisting of semiconductor perylenetetracarboxylic dianhydride, semiconductor perylene diimide, semiconductor dioctylbenzothiophene-benzothiophene, and N,N'-dimethyldicarboximide.
4. The boron nitride encapsulated two-dimensional organic-inorganic heterojunction according to claim 1, characterized in that: The gold electrode is made by electron beam exposure technology, and a hollow square hole with a side length of 20 um is arranged on the gold electrode.
5. The boron nitride encapsulated two-dimensional organic-inorganic heterojunction according to claim 1, characterized in that: After the gold electrode is covered on the boron nitride, it is heated in a vacuum at 200-260°C.
6. The boron nitride encapsulated two-dimensional organic-inorganic heterojunction according to claim 1, characterized in that: The two-dimensional inorganic material to be transferred is obtained by a mechanical exfoliation method to obtain a two-dimensional inorganic material on silicon oxide.
7. The boron nitride encapsulated two-dimensional organic-inorganic heterojunction according to claim 1, characterized in that: The tip of the fine needle is dipped in a metal glue which is liquid at room temperature and serves as glue for bonding the gold electrode.
Citation Information
Patent Citations
Boron nitride packaged two-dimensional organic-inorganic heterojunction
CN210467888U
Method of manufacturing graphene substrate, and graphene substrate
US20130272951A1
Direct formation of hexagonal boron nitride on silicon based dielectrics
US20190097000A1