A PN junction piezoresistive diffused silicon pressure sensor and manufacturing method thereof
By using epitaxial instead of injection in diffusion silicon pressure sensors, combined with photolithography and oxidation processes, the problems of difficulty in manufacturing the resistor strip and thin protective layer of the device are solved, and higher reliability and yield are achieved, improving the device's impact resistance Wear characteristics and sensitivity.
Patent Information
- Application Number
- CN201911288464.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-12-16
AI Technical Summary
During the production process, the existing diffusion silicon pressure sensors have problems such as difficult to make the resistive strip, thin device protective layer, and easy to breakdown in the PN junction shape, which affects its reliability and yield.
Epitaxial instead of injection, the Si epitaxial layer is grown by high temperature, combined with photolithography, etching, oxidation and nitriding processes to form a homogeneous PN junction, and an oxide layer or nitriding layer is deposited on the surface of the device for protection, adjusting the shape of the PN junction To improve device reliability.
The preparation process is simplified, the design difficulty is reduced, the reliability and breakdown resistance of the device are improved, and the yield and sensitivity are improved.
Smart Images

Figure CN110823422B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of microelectronics technology, and in particular to a PN junction piezoresistive diffused silicon pressure sensor with simple process and high reliability and a manufacturing method thereof. The method can be used to prepare a PN junction piezoresistive diffused silicon pressure sensor and a SOI piezoresistive diffused silicon pressure sensor. Background Art
[0002] Diffused silicon pressure sensors have attracted much attention from the industry due to their large output signal, simple processing circuit, and ability to measure multi-faceted parameters such as pressure and differential pressure. They have developed rapidly in the past decade and have a considerable share in the sensor and transmitter market. Developed countries abroad have conducted in-depth research on the mechanism and application of diffused silicon pressure sensors based on their strong semiconductor industry foundation and have achieved a lot of results. However, in the production process of existing diffused silicon pressure sensors, the method of injection and then diffusion is used for the production of resistance bars. Since strict annealing is required after injection, there are problems such as lateral diffusion after annealing, which increases the difficulty of design. In addition, due to the limitations of the injection process, the protective layer of the device is very thin and has poor protection for the device. At the same time, since the shape of the PN junction formed after injection is fixed, the surface is easy to break down, which affects the reliability and production yield of the device. Summary of the invention
[0003] The present invention aims to solve the problems of existing diffused silicon pressure sensors and to provide a PN junction piezoresistive diffused silicon pressure sensor with simple process and high reliability and a manufacturing method thereof.
[0004] To achieve the above object, the technical solution adopted by the present invention is:
[0005] 1. A method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor, characterized in that the manufacturing method comprises the following steps:
[0006] (1) Epitaxy: first select a substrate with a resistivity of 1-20Ω*cm, and grow a 0.5-4um Si epitaxial layer at a high temperature of 1000-1150℃; the epitaxial layer is inversely proportional to the substrate, and the growth is P-type, and the substrate is selected as N-type to form a uniform PN junction. The growth pressure is 10-760 Torr, and the chloroform flow rate is 40-1000 cubic centimeters per minute;
[0007] (2) Photolithography: The PN junction is coated with glue by a spin coating method at a rotation speed of 1500-4000 rpm, and then baked on a hot plate for 30-120 seconds. After baking, it is exposed for 15-60 seconds, developed for 10-90 seconds, and hardened for 25-60 minutes to carve out device patterns of smooth-edged barrier strips and pressure-bonded points;
[0008] (3) Etching: etching the PN junction after photolithography to realize the pattern obtained by photolithography, with an etching depth of 1-4.5 μm, and using wet or dry etching. When wet etching is used, the etchant is HNO3+HF in a ratio of 3:1-1:4, and the etching is carried out for 3-15 minutes; when dry etching is used, Cl2 is selected as the etchant to form a three-dimensional table PN junction;
[0009] (4) After removing the photoresist from the three-dimensional mesa PN junction, the three-dimensional mesa PN junction is oxidized or nitrided. When oxidation is selected, a 1-2 um oxide layer is grown on the three-dimensional mesa PN junction using dry oxygen-wet oxygen-dry oxygen oxidation conditions, the temperature is 850-1150°C, the O2 flow rate is 50-430 cubic centimeters per minute, and the water vapor flow rate is 60-350 cubic centimeters per minute; when nitridation is selected, a layer of silicon nitride is grown using LPCVD (low pressure chemical vapor deposition) or PECVD (plasma enhanced chemical vapor deposition) For device protection; if LPCVD is used to grow silicon nitride, the temperature is 500-850°C, the NH3 flow rate is 100-500 cubic centimeters / minute, and the SIH4 flow rate is 50-400 cubic centimeters / minute; if PEVD is used for growth, the RF high-frequency power is 100-600W, the low-frequency power is 200-500W, the NH3 flow rate is 100-300 cubic centimeters / minute, the SIH4 flow rate is 50-400 cubic centimeters / minute, and the N2 flow rate is 3000-8000 cubic centimeters / minute;
[0010] (5) After device protection, photolithography of solder joints, select negative photoresist, apply the photoresist at a speed of 1500-4000 rpm, then bake on a hot plate for 30-120s, expose for 15-60s after baking, develop for 10-90s, harden for 25-60 minutes, photolithograph the solder joint area, and then remove the oxide layer in the area;
[0011] (6) Depositing a metal electrode on the solder joint where the oxide layer has been removed, the electrode material is Al / Cr-Ni-Au, and then placing it in a degumming solution to dissolve the metal on the photoresist area, and retaining the electrode in the solder joint area. The thickness of the Al / Cr-Ni-Au metal is 0.8-2um;
[0012] (7) Alloying: annealing the entire wafer after metal deposition at 400-750°C for 20-60 min to alloy and obtain ohmic contact;
[0013] (8) Making thin Al / conductive polysilicon, depositing thin Al / conductive polysilicon on the front side of the alloyed wafer to cover the barrier device, keeping the upper and lower potentials of the barrier device consistent;
[0014] (9) Anisotropic etching of the silicon cup on the back side: The back side of the above-mentioned wafer is etched with potassium hydroxide or tetramethylammonium hydroxide as an etchant. The concentration of the etching solution is 10-45%. After etching, it is electrostatically sealed with glass to obtain a finished diffused silicon pressure sensor. The electrostatic sealing temperature is 300-500°C and the voltage is 100-500V.
[0015] The present invention comprises: in step (1), the doping concentration of the grown epitaxial layer is 2-4.5*10 17 cm-3, or 3-5.5*10 19 cm-3.
[0016] The present invention also includes: in step (2), the rotation speed during the gluing process is optimized to 3500-4000 rpm, and the exposure time is optimized to 15-30s.
[0017] The PN junction piezoresistive diffused silicon pressure sensor of the present invention comprises a wafer, and is characterized in that raised resistance strip devices and pressure welding points are distributed on the wafer, electrodes are also covered on the top of the resistance strip devices, and an oxygen layer or a nitride layer is also provided on the outer surface of the wafer and the pressure welding points.
[0018] The barrier strip device described in the present invention is a snake-type structure.
[0019] The edge shape of the barrier strip device of the present invention is a rounded structure to avoid tip discharge, thereby further improving the breakdown performance of the device.
[0020] The beneficial effects and design principles of the present invention are as follows:
[0021] Beneficial Effects
[0022] 1: The preparation process is simple and the process window is large;
[0023] (1) Since the present invention uses epitaxy instead of implantation, there is no problem of lateral diffusion, and the precise diffusion process is eliminated, which reduces the difficulty of preparation in both design and process. Under the conventional preparation process, annealing and diffusion are required after implantation. The temperature and time of this step must be precisely controlled, and the process window is very narrow. At the same time, lateral diffusion is inevitable after diffusion, which is also greatly affected by the annealing temperature and time. Due to the existence of lateral diffusion, diffusion margin must be left in the design, which makes the design more difficult.
[0024] (2) In terms of design, using epitaxy instead of implantation can more easily realize low-concentration design. At present, the implantation concentration of diffused silicon pressure sensors is divided into two designs: high concentration and low concentration. In the high-concentration design, the implantation and annealing processes are simple, but the sensitivity is low and a long resist strip is required. In the low-concentration design, the implantation and annealing process requirements are very high and three implantations are required, but the lithography and related processes are relatively simple and the sensitivity is higher.
[0025] 2: High product reliability;
[0026] (1) The doping concentration of the device layer of the present invention is uniformly distributed, and the device performance is more stable. The impurities after injection are Gaussian distributed, and there is a maximum doping concentration. It must be diffused again to make it as evenly distributed as possible. The annealing and re-expansion process is very critical. If there is a little fluctuation, the product performance will be affected. The impurity concentration after epitaxy is uniformly distributed, and there is no risk in this regard.
[0027] (2) The device layer of the present invention is better protected. The barrier strip made by epitaxy can be protected by a thicker oxide layer or nitride layer on top, which can be as thick as 1-2um, while the barrier strip made by injection can only be protected by an oxide layer of about 1000A. Therefore, the sensor made by the present invention has higher reliability. Figure 5 shown.
[0028] (3) The device layer of the present invention has better anti-breakdown characteristics. In the traditional process, the PN junction has a large area and a fixed shape, which is easy to break down, especially at the surface. Since the present invention does not use injection, the shape of the PN junction can be adjusted to avoid tip discharge and thus improve the breakdown characteristics. In addition, since most of the barrier strips of the present invention are protected by the oxide layer, the PN junction area is greatly reduced, and the surface that is easy to break down in the traditional process has been protected by the oxide layer, so the breakdown characteristics are further improved.
[0029] (4) The device layer of the present invention has better single crystal quality. Since the traditional device layer is obtained by implantation, high-energy implantation will inevitably bring a large number of lattice defects. Although it has been repaired, it is difficult to repair it to a single crystal state, which affects the performance and reliability of the device. The present invention uses epitaxy instead of implantation to grow a single crystal layer as a device, and its reliability and sensitivity are better than those of traditional methods.
[0030] Design Principle
[0031] The design principle of the present invention is based on the sensor principle - the piezoresistive effect of doped silicon. In order to obtain a pressure sensor that meets the requirements, the doping concentration of the resistor strip needs to be precisely controlled. The traditional method is to use the injection diffusion method, but injection diffusion has many problems. The present invention also uses the epitaxial method to precisely control the doping concentration, avoiding the problems caused by the traditional injection method. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A schematic diagram of the manufacturing process of the pressure sensor of the present invention;
[0033] Figure 2 A schematic diagram of the preparation process of the pressure sensor in the comparative example;
[0034] Figure 3 It is a comparison curve diagram of the pressure characteristics of the sensor of the present invention;
[0035] Figure 4 It is a schematic diagram of the cross-sectional structure of a PN junction according to the present invention;
[0036] Figure 5 For the present invention Figure 4 The A-axis outline in the figure is an enlarged schematic diagram;
[0037] Figure 6 For the present invention Figure 4 Schematic diagram of the cross section along the dotted line B;
[0038] Figure 7 Comparison of the breakdown voltage of 11 groups of devices between the conventional method and the present invention;
[0039] Figure 8 The figure shows the comparison of eight wafer yields between the conventional method and the present invention.
[0040] Description of the main figure numbers in the figure: Figure 1 In the middle: 1 is a wafer; 2 is an epitaxial layer; 3 is a bonding pad; 4 is a barrier strip device; 5 is a protective oxide layer or nitride layer; 6 is a photoresist left by photolithography in the bonding pad area; 7 is an electrode; Figure 2 Middle: 8 is a wafer; 9 is an oxide layer; 10 is a resist; 11 is a bonding point; 12 is a shielding layer; 13 is a shielding layer; 14 is an electrode. DETAILED DESCRIPTION
[0041] In order to more clearly illustrate the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Example 1
[0043] The present invention is a method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor with simple process and high reliability. The method comprises epitaxy, photolithography, etching, oxidation, metallization and other processes. The process flow is as follows: Figure 1 The specific process is as follows
[0044] (1) Epitaxy: First, select an N-type wafer 1 with a resistivity of 1-20Ω*cm as the substrate, and grow a 0.5-4um Si epitaxial layer 2 at a high temperature of 1000-1150℃; the epitaxial layer 2 is inversely proportional to the N-type wafer 1, and grows a P-type. The substrate is selected to be N-type to form a uniform PN junction. The growth pressure is 10-760 Torr, the chloroform flow rate is 3500-1000 cubic centimeters per minute, and the doping concentration of the grown epitaxial layer is 2~4.5*10 17 cm-3;
[0045] (2) Photolithography: the PN junction is coated with glue by a spin coating method at a rotation speed of 1500-4000 rpm, and then baked on a hot plate for 30-120 seconds, exposed for 15-60 seconds after baking, developed for 10-90 seconds, and hardened for 25-60 minutes, and the barrier strip device 4 with smooth edges and the device's pressure welding point 3 are engraved;
[0046] (3) Etching: etching the PN junction after photolithography to realize the pattern obtained by photolithography, with an etching depth of 1-4.5 μm, and using wet or dry etching. When wet etching is used, the etchant is HNO3+HF in a ratio of 3:1-1:4, and the etching is carried out for 3-15 minutes; when dry etching is used, Cl2 is selected as the etchant to form a three-dimensional table PN junction;
[0047] (4) removing the photoresist from the three-dimensional mesa PN junction and then oxidizing or nitriding it. When oxidation is selected, a 1-2 μm protective oxide layer 5 is grown on the three-dimensional mesa PN junction using dry oxygen-wet oxygen-dry oxygen oxidation conditions, the temperature is 850-1150° C., the O2 flow rate is 50-430 cubic centimeters per minute, and the water vapor flow rate is 60-350 cubic centimeters per minute. When nitriding is selected, LPCVD (low pressure chemical vapor deposition) or PECVD (plasma enhanced chemical vapor deposition) is used to grow a layer of silicon nitride for Nitride layer for device protection; if LPCVD is used to grow silicon nitride, the temperature is 500-850°C, the NH3 flow rate is 100-500 cubic centimeters per minute, and the SIH4 flow rate is 50-400 cubic centimeters per minute; if PEVD is used for growth, the RF high-frequency power is 100-600W, the low-frequency power is 200-500W, the NH3 flow rate is 100-300 cubic centimeters per minute, the SIH4 flow rate is 50-400 cubic centimeters per minute, and the N2 flow rate is 3000-8000 cubic centimeters per minute;
[0048] (5) After device protection, photolithography of the solder joints, select negative photoresist, and apply the photoresist at a speed of 1500-4000 rpm, then bake on a hot plate for 30-120s, expose for 15-60s after baking, develop for 10-90s, and harden for 25-60 minutes. Photolithography the photoresist 6 pattern left in the solder joint area, and then remove the oxide layer in this area;
[0049] (6) Depositing a metal electrode on the bonding pad where the oxide layer has been removed, the electrode material is Al / Cr-Ni-Au, and then placing it in a degumming solution to dissolve the metal on the photoresist area, and retaining the electrode 7 in the bonding pad area. The thickness of the Al / Cr-Ni-Au metal is 0.8-2 um;
[0050] (7) Alloying: annealing the entire wafer after metal deposition at 400-750°C for 20-60 min to alloy and obtain ohmic contact;
[0051] (8) Make thin Al / conductive polysilicon, deposit thin Al / conductive polysilicon on the front side of the alloyed wafer to cover the barrier strip, and keep the upper and lower potentials of the barrier strip consistent;
[0052] (9) Anisotropic etching of the silicon cup on the back side: The back side of the above-mentioned wafer is etched with potassium hydroxide or tetramethylammonium hydroxide as an etchant. The concentration of the etching solution is 10-45%. After etching, it is electrostatically sealed with glass to obtain a finished diffused silicon pressure sensor. The electrostatic sealing temperature is 300-500°C and the voltage is 100-500V.
[0053] The PN junction piezoresistive diffused silicon pressure sensor formed by the present invention has a finished structure comprising a wafer 1, on which are distributed raised resistance bar devices 4 and pressure welding points 3, and the resistance bar devices are of a serpentine structure on the wafer; the top of the resistance bar devices is also covered with electrodes 7, and an oxygen layer or a nitride layer 5 is also provided on the outer surface of the wafer 1 and the pressure welding points 3.
[0054] Example 2
[0055] 1: First, select an N-type wafer 1 with a resistivity of 1-4Ω*cm, and grow a P-type epitaxial layer 2 at 1000-1150℃ with a doping concentration of 4*10 19 cm -3 , thickness is 0.5-4um, growth pressure is 55 torr, chloroform flow rate is 95 cubic centimeters per minute, and the doping concentration of the grown epitaxial layer is 3-5.5*10 19 cm-3.
[0056] The remaining steps are the same as those in Example 1 and are therefore omitted.
[0057] Comparative Example 1:
[0058] 1: First, select an N-type wafer with a resistivity of 1-4Ω*cm8, oxidize the wafer, and grow an oxide layer of about 1.2um using the conventional oxidation conditions of dry oxygen-wet oxygen-dry oxygen9
[0059] 2: Photolithography, using positive photolithography, with a rotation speed of 4000 rpm for 40 seconds and an exposure time of 15 seconds, to carve out device patterns such as the resistance bar 10 and the pressure welding point 11, and then use wet etching to remove the oxide layer at the resistance bar and the pressure welding point
[0060] 3: Oxidation: The wafer is oxidized again. The oxidation condition is to use dry oxygen at 1150° C. to grow an oxide layer of about 1000 Å for the implanted shielding layers 12 and 13 .
[0061] 4: Injection, inject B atoms, the dose is 4*10 19 cm -3
[0062] 5: Annealing diffusion, temperature is 1000℃, annealing for 30min,
[0063] 6: Photolithography of lead holes, negative photoresist, rotation speed 4000 rpm for 40s, exposure time 15s, photolithography of the solder joint area, and then wet etching to remove the oxide layer in the area
[0064] 7: Deposit metal electrodes. Use magnetron sputtering equipment to deposit Al with a thickness of 1.2um. Then put it into a degumming solution for degumming. The metal on the photoresist area is dissolved, and the electrode 14 in the pad area is retained.
[0065] 8: Alloy, put the whole wafer into: 550℃ annealing for 30min to alloy and obtain ohmic contact
[0066] 9: Make a thin Al layer, cover it on the barrier strip, keep the upper and lower potentials of the barrier strip consistent, and the thickness is about 1000A
[0067] 10: Anisotropically etch the silicon cup on the back and then electrostatically seal it with the glass.
[0068] Implementation Effect
[0069] Depend on Figure 3 It can be seen that the pressure output of the pressure sensor made by the present invention meets the requirements of the pressure linear output characteristics of the pressure sensor made by the traditional process, but the sensitivity of the pressure sensor made by the present invention is higher. This is because there is more lattice damage in the silicon wafer after injection, which is not completely repaired in the subsequent annealing repair, and there are still some defects in the device area. Defects reduce sensitivity. In the present invention, since epitaxy is used instead of injection, the device layer is a single crystal grown by epitaxy, and the defects are greatly reduced, so the sensitivity of the present invention is higher.
[0070] Depend on Figure 4 and Figure 5 and Figure 6 It can be seen that the device made by the present invention has a three-dimensional table PN junction structure, and the outline avoids sharp corners. This structure can improve the breakdown characteristics of the PN junction and make the device more stable.
[0071] In terms of yield, Figure 7 It can be seen that the yield rate of the present invention has been significantly improved and is more stable. This is due to the following reasons:
[0072] (1) Better protection effect of barrier devices. Since the traditional injection method can only have a 1000A oxide layer to protect the device, its protection ability is poor and its anti-interference ability is not strong. There is a risk of insufficient protection leading to device failure in the product process. However, the present invention can use a 1-2um oxide layer for protection, which has strong anti-interference ability and no risk of insufficient protection.
[0073] (2) The process is simpler. Since the traditional injection process must be annealed and diffused after injection, the temperature and time must be controlled very precisely. If there is a fluctuation in the control, it will cause changes in the doping concentration of the barrier device and the size of the barrier, resulting in device failure. In addition, the requirements for the oxide layer as an injection shielding layer are also very high. If the thickness of the shielding layer changes, it will directly affect the junction depth of the PN junction and affect the performance. Under the present invention, there is no such strict process requirement, the product is simpler to process, the manufacturing window is large, and the yield will naturally be higher.
[0074] (3) The breakdown voltage is improved and the PN junction is more stable. The PN junction under the traditional structure is formed by injection annealing, and its shape is fixed. There is a problem of tip discharge, and the breakdown position is often on the surface. The shape of the PN junction of the device made by the present invention can be controlled by the photolithography process, and the periphery is protected by an oxide layer, which avoids the problems of tip discharge and surface breakdown, and further improves the product yield.
Claims
1. A method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor, characterized in that: The preparation method comprises the following steps: (1) Epitaxy: first select a substrate with a resistivity of 1-20Ω*cm, and grow a 0.5-4um Si epitaxial layer at a high temperature of 1000-1150℃; the epitaxial layer is inversely proportional to the substrate, and the P type is grown. The substrate is selected to be N type to form a uniform PN junction. The growth pressure is 10-760 Torr, and the chloroform flow rate is 40-1000 cubic centimeters per minute; (2) Photolithography: The PN junction is coated with glue by a spin coating method at a rotation speed of 1500-4000 rpm, and then baked on a hot plate for 30-120 seconds. After baking, it is exposed for 15-60 seconds, developed for 10-90 seconds, and hardened for 25-60 minutes to carve out device patterns of smooth-edged barrier strips and pressure-bonded points; (3) Etching: etching the PN junction after photolithography to realize the pattern obtained by photolithography, with an etching depth of 1-4.5 μm, and using wet or dry etching. When wet etching is used, the etchant is HNO3+HF in a ratio of 3:1-1:4, and the etching is carried out for 3-15 minutes; when dry etching is used, Cl2 is selected as the etchant to form a three-dimensional table PN junction; (4) After removing the photoresist from the three-dimensional mesa PN junction, oxidize or nitride it. When oxidation is selected, the three-dimensional mesa PN junction is oxidized by dry oxygen-wet oxygen-dry oxygen to grow an oxide layer of about 1-2 um, the temperature is 850-1150°C, the O2 flow rate is 50-430 cubic centimeters / minute, and the water gas flow rate is 60-350 cubic centimeters / minute; when nitridation is selected, LPCVD or PECVD is used to grow a layer of silicon nitride for device protection; if LPC is used VD growth of silicon nitride, temperature is 500-850℃, NH3 flow rate is 100~500 cubic centimeters / minute, SIH4 flow rate is 50~400 cubic centimeters / minute; if PEVD growth is adopted, RF high frequency power is 100~600W, low frequency power is 200~500W, NH3 flow rate is 100~300 cubic centimeters / minute, SIH4 flow rate is 50~400 cubic centimeters / minute, N2 flow rate is 3000~8000 cubic centimeters / minute; (5) After device protection, photolithography of solder joints, select negative photoresist, apply the photoresist at a speed of 1500-4000 rpm, then bake on a hot plate for 30-120s, expose for 15-60s after baking, develop for 10-90s, harden for 25-60 minutes, photolithograph the solder joint area, and then remove the oxide layer or nitride layer in the area; (6) depositing a metal electrode on the welding spot where the oxide layer is removed, wherein the electrode material is Al or Cr-Ni-Au, and then placing the electrode in a degumming solution to dissolve the metal on the photoresist area, and retaining the electrode in the welding spot area, wherein the thickness of the Al or Cr-Ni-Au metal is 0.8-2 um; (7) Alloying: annealing the entire wafer after metal deposition at 400-750°C for 20-60 min to alloy and obtain ohmic contact; (8) Making thin Al or conductive polysilicon, depositing thin Al or conductive polysilicon on the front side of the alloyed wafer to cover the barrier device, keeping the upper and lower potentials of the barrier device consistent; (9) Anisotropic etching of the silicon cup on the back side: The back side of the above-mentioned wafer is etched with potassium hydroxide or tetramethylammonium hydroxide as an etchant. The concentration of the etching solution is 10-45%. After etching, it is electrostatically sealed with glass to obtain a finished diffused silicon pressure sensor. The electrostatic sealing temperature is 300-500°C and the voltage is 100-500V.
2. The method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor according to claim 1, characterized in that: In step (1), the doping concentration of the grown epitaxial layer is 2~4.5*10 17 cm -3 , or 3-5.5*10 19 cm -3 .
3. The method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor according to claim 1, characterized in that: In step (2), the rotation speed during the gluing process is 3500-4000 rpm, and the exposure time is 15-30 s.
4. The method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor according to claim 1, characterized in that: The PN junction piezoresistive diffused silicon pressure sensor comprises a wafer, on which are distributed raised resistance strip devices and pressure welding points, electrodes are also covered on the top of the resistance strip devices, and an oxygen layer or a nitride layer is also provided on the outer surface of the wafer and the pressure welding points.
5. The method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor according to claim 1, characterized in that: The barrier strip device is a snake-shaped structure.
6. The method for manufacturing a PN junction piezoresistive diffused silicon pressure sensor according to claim 1 or 4, characterized in that: The edge shape of the barrier strip device is a rounded structure to avoid tip discharge.