Method and device for preparing composite plate by extrusion-rolling composite

Through the extrusion-rolling composite sheet method, the extrusion mold structure of asymmetric grooves and bump cavity is used to solve the problems of interface defects and insufficient bonding force, and high-quality composite sheet preparation is achieved, simplifying the process And reduce costs.

CN110842046BActive Publication Date: 2024-11-01HUNAN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911313081.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-18
Publication Date
2024-11-01
Estimated Expiration
2039-12-18

AI Technical Summary

Technical Problem

In the existing composite sheet preparation methods, the problem of interface defects and insufficient bonding force is difficult to achieve high-quality interface bonding, especially when preparing double-layer and multi-layer composite materials.

Method used

An extrusion-rolling device consisting of a concave blank extrusion die and a convex blank extrusion die is used to generate external convex and internal concave blanks through extrusion, and roll them under preheating of the heating device to form composite sheets. Asymmetric groove and bump cavity structures to enhance the bonding force and composite area of ​​the blank.

Benefits of technology

The removal of grease and oxide layer treatment steps are reduced, the bonding force and strength of the composite material are improved, three-dimensional composite is realized, mold structure and operation are simplified, cost is reduced, and the quality of the board and industrial production capacity are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110842046B_ABST
    Figure CN110842046B_ABST
Patent Text Reader

Abstract

The present invention discloses a method and device for preparing a composite plate by extrusion-rolling composite. The method comprises homogenizing a metal blank, preparing an inner concave blank by extrusion using a concave blank extrusion die, preparing an outer convex blank by extrusion using a convex blank extrusion die, extruding the outer convex blank into an inner concave blank of equal length and width to obtain a composite blank and rolling treatment. The device is composed of a concave blank extrusion die and a convex blank extrusion die, and the two sets of molds are composed of an extrusion head, an upper module, a lower module, a heating device, a temperature measuring device, and a fastening device. The upper module matches the lower module and is fixed by a fastening device. One side of the space formed between the upper module and the lower module matches the extrusion head, and the other side is an extrusion working area. A heating device and a temperature measuring device are arranged on the upper module or / and the lower module. The mold structure of the present invention is simple, and three-dimensional composite materials can be realized through the outer convex blank and the inner concave blank. The bonding force between the matrix materials is stronger, the operation is convenient, the cost is low, and industrialization can be well realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of processing metal composite materials, and in particular relates to a method and a device for preparing a composite plate by extrusion-rolling composite. Background Art

[0002] Composite materials are made of multiple materials with different properties. They have incomparable advantages over single metal materials. Through reasonable material selection and appropriate combination, they can not only retain the inherent characteristics of the constituent materials, but also complement each other through the composite effect, so that the composite board has excellent comprehensive performance. Chinese inventions CN106623424A, CN106862271A, etc. disclose methods for preparing laminated composite plates. The interfaces of the composite plates prepared by these methods are planes. Chinese invention CN110303079A discloses a method for cross-corrugation rolling of a bimetallic composite plate, and prepares a bimetallic composite plate with a cross-corrugated interface; Chinese invention CN110238196A discloses a method for longitudinal wave rolling of a three-layer metal composite plate strip, and a composite plate blank is rolled by a corrugation roller mill to obtain a three-layer finished composite plate with a corrugated bonding interface; Chinese invention CN109731912A discloses a method for rolling and preparing a toothed bonding surface of a titanium / aluminum / magnesium composite plate, and a toothed surface is rolled on a rolling mill with a toothed roller to prepare a composite plate. The interface of the composite plate prepared by these patents is a curved surface, which increases the bonding force between the component materials to a certain extent. Summary of the invention

[0003] The object of the present invention is to provide a method and device for preparing a composite plate by extrusion-rolling composite.

[0004] The technical solution of the present invention is:

[0005] A device for preparing composite plates by extrusion-rolling composite, which consists of a concave billet extrusion die and a convex billet extrusion die. The two sets of dies are composed of an extrusion head, an upper module, a lower module, a heating device, a temperature measuring device, and a fastening device. The upper module matches the lower module and is fixed by the fastening device. One side of the space formed between the upper module and the lower module matches the extrusion head, and the other side is an extrusion working area. The upper module and / or the lower module are provided with a heating device and a temperature measuring device.

[0006] Furthermore, the lower module of the concave extrusion die has one or more concave groove forming blocks, and the lower module of the convex extrusion die has one or more convex block cavities, and the number of the concave groove forming blocks is equal to the number of the convex block cavities.

[0007] Furthermore, the groove forming block and the protrusion cavity have equal bevel angles, and the angle between them and the horizontal line is 45 degrees. 。 -90 。 .

[0008] Furthermore, the size of the convex block cavity is slightly larger than that of the concave block cavity, and the cavity widths of the concave extrusion die and the convex extrusion die are equal.

[0009] A method for preparing a composite plate by extrusion-rolling composite using the above device comprises the following steps:

[0010] (1) Performing homogenization treatment on the metal blanks respectively;

[0011] (2) using a concave billet extrusion die to extrude an inner concave billet of a composite billet;

[0012] (3) Extruding a convex blank of the composite blank using a convex blank extrusion die;

[0013] (4) Extruding the convex blank obtained by extrusion into the concave blank to obtain a composite blank;

[0014] (5) The composite blank is rolled to obtain a composite plate.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. The method of the present invention generates a new metal surface by extrusion, which can reduce the steps of removing grease and oxide layer before the common composite method. The generated new metal surface can be more conducive to extrusion and rolling composite, and the bonding force of the composite material is good;

[0017] 2. The convex size of the convex blank is slightly larger than the concave size of the concave blank, which can combine the two blanks and reduce composite interface defects;

[0018] 3. The convex blank and the concave blank can realize three-dimensional composite material, increasing the blank composite area and composite strength;

[0019] 4. The composite interface of the composite blank can be improved by designing groove forming blocks and convex cavity with different shapes, and double-layer and multi-layer composite materials can be prepared;

[0020] 5. The extrusion die of the present invention has a simple structure, is easy to operate and has low cost;

[0021] 6. The device of the present invention is provided with a heating device to realize preheating treatment before extrusion and improve the plastic deformation ability of the plate. The temperature of the plate can be collected by a thermocouple and transmitted to an external temperature measuring device for detection, and the collected data is transmitted to an external computer system for temperature control.

[0022] 7. The method of the present invention can prepare large-scale composite plates with strong interface bonding ability and high plate quality through extrusion and rolling, and can better realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Flow chart of the method of the present invention.

[0024] Among them: 1. lower module, 2. heating device, 3. temperature measuring device, 4. upper module, 5. fastening device, 6. extrusion head.

[0025] Figure 2 It is a structural schematic diagram of the lower module of the convex blank extrusion die, wherein: 11. Convex block cavity.

[0026] Figure 3 It is a structural schematic diagram of the lower module of the concave billet extrusion die, wherein: 12. Groove forming block.

[0027] Figure 4 Schematic diagram of the convex blank.

[0028] Figure 5 Schematic diagram of the concave blank. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0030] like Figures 1 to 3 As shown, the device of the present invention is composed of a concave billet extrusion die and a convex billet extrusion die. Both sets of molds are composed of a lower module 1, a heating device 2, a temperature measuring device 3, an upper module 4, a fastening device 5, and an extrusion head 6. The upper module 4 matches the lower module 1 and is fixed by the fastening device 5. One side of the space formed between the upper module 4 and the lower module 1 matches the extrusion head 6, and the other side is the extrusion working area. The heating device 2 and the temperature measuring device 3 are arranged on the upper module 4 and / or the lower module 1; the convex billet extrusion die has one or more convex block cavities 11, and the lower module of the concave billet extrusion die has one or more groove forming blocks 12. The number of groove forming blocks 12 and the convex block cavities 11 is equal, and the size of the convex block cavity 11 is slightly larger than that of the groove forming block 12. The prepared convex billet is as follows: Figure 4 , concave blanks such as Figure 5 As shown;

[0031] Example 1

[0032] The 7055 and 7N01 aluminum alloy billets with an initial thickness of 10 mm were extruded and rolled to prepare 2 mm thick composite plates. The lower module 1 of the concave billet extrusion die had a groove forming block, and the lower module 1 of the convex billet extrusion die had a convex block cavity 11. The angle between the groove forming block 12 and the convex block cavity 11 and the horizontal line was 60. 。 .

[0033] (1) The 7055 aluminum alloy billet was homogenized at 400℃ / 12h+465℃ / 24h, and the 7N01 aluminum alloy billet was homogenized at 470℃ / 24h;

[0034] (2) starting the heating device 2, raising the temperature of the concave billet extrusion die to 420° C., and extruding an inner concave 7N01 aluminum alloy billet to prepare a composite billet;

[0035] (3) starting the heating device 2, raising the temperature of the convex billet extrusion die to 420° C., and extruding an outer convex 7055 aluminum alloy billet to prepare a composite billet;

[0036] (4) extruding the convex 7055 aluminum alloy billet obtained by extrusion into the concave 7N01 aluminum alloy billet to obtain a composite billet;

[0037] (5) The composite blank is preheated to 420°C and kept at this temperature for 30 minutes, and the composite blank is rolled to prepare a composite plate.

[0038] Example 2

[0039] The AZ31 magnesium alloy and 7050 aluminum alloy billets with an initial thickness of 10 mm were extruded and rolled to prepare a 3 mm thick composite plate. The lower module 1 of the concave billet extrusion die has a groove forming block, and the lower module 1 of the convex billet extrusion die has a convex block cavity 11. The angle between the groove forming block 12 and the convex block cavity 11 and the horizontal line is 70 。 .

[0040] (1) The 7050 aluminum alloy was homogenized at 470°C / 24h, and the AZ31 magnesium alloy was homogenized at 415°C / 15h;

[0041] (2) starting the heating device 2, raising the temperature of the concave billet extrusion die to 420° C., and extruding the concave 7050 aluminum alloy billet to prepare the composite billet;

[0042] (3) starting the heating device 2, raising the temperature of the convex billet extrusion die to 400° C., and extruding an outer convex AZ31 magnesium alloy billet to prepare a composite billet;

[0043] (4) extruding the convex AZ31 magnesium alloy billet obtained by extrusion into the concave 7050 aluminum alloy billet to obtain a composite billet;

[0044] (5) The composite blank is preheated to 400°C and kept at this temperature for 30 minutes, and the composite blank is rolled to prepare a composite plate.

[0045] Example 3

[0046] The 7055 and 7N01 aluminum alloy billets with an initial thickness of 10 mm were extruded and rolled to prepare 2 mm thick composite plates. The lower module 1 of the concave billet extrusion die had three concave forming blocks, and the lower module 1 of the convex billet extrusion die had three convex block cavities 11. The angle between the concave forming block 12 and the convex block cavity 11 and the horizontal line was 80. 。 .

[0047] (1) The 7055 aluminum alloy billet was homogenized at 400℃ / 12h+465℃ / 24h, and the 7N01 aluminum alloy billet was homogenized at 470℃ / 24h;

[0048] (2) starting the heating device 2, raising the temperature of the concave billet extrusion die to 420° C., and extruding an inner concave 7N01 aluminum alloy billet to prepare a composite billet;

[0049] (3) starting the heating device 2, raising the temperature of the convex billet extrusion die to 420° C., and extruding an outer convex 7055 aluminum alloy billet to prepare a composite billet;

[0050] (4) extruding the convex 7055 aluminum alloy billet obtained by extrusion into the concave 7N01 aluminum alloy billet to obtain a composite billet;

[0051] (5) The composite blank is preheated to 420°C and kept at this temperature for 30 minutes, and the composite blank is rolled to prepare a composite plate.

Claims

1. A method for preparing a composite sheet by extrusion-rolling composite, It is characterized in that The steps include: (1) Performing homogenization treatment on the metal blanks respectively; (2) starting the heating device, heating the concave billet extrusion die to 420° C., and extruding an inner concave billet of the composite billet; (3) starting the heating device, raising the temperature of the convex billet extrusion die to 420° C., and extruding an outer convex billet of the composite billet; (4) Extruding the convex blank obtained by extrusion into the concave blank to obtain a composite blank; (5) rolling the composite blank to obtain a composite plate; The device used in the method is composed of a concave billet extrusion die and a convex billet extrusion die. Both sets of dies are composed of an extrusion head, an upper module, a lower module, a heating device, a temperature measuring device, and a fastening device. The upper module matches the lower module and is fixed by the fastening device. One side of the space formed between the upper module and the lower module matches the extrusion head, and the other side is an extrusion working area. The upper module and / or the lower module are provided with a heating device and a temperature measuring device. The groove forming block and the convex block cavity have equal bevel angles, and the angle with the horizontal line is 45 。 -90 。 ; The size of the convex block cavity is slightly larger than that of the concave block, and the cavity widths of the concave and convex extrusion dies are equal; The lower module of the concave billet extrusion die has one or more than two concave molding blocks, and the lower module of the convex billet extrusion die has one or more than two convex block cavities, and the number of the concave molding blocks is equal to that of the convex block cavities.