A roller-bottom continuous solution heat treatment equipment and process for aluminum alloy long profiles

By designing roller-bottom continuous solution heat treatment equipment for long aluminum alloy profiles, the problems of poor temperature control and low production efficiency in traditional processes are solved, efficient temperature control and continuous production are achieved, and product quality and production efficiency are improved. Reduced costs.

CN110894571BActive Publication Date: 2024-11-22ARES IND FURNACE TIANJIN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811061730.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-09-12
Publication Date
2024-11-22
Estimated Expiration
2038-09-12

AI Technical Summary

Technical Problem

The traditional solid solution heat treatment process poorly controls the temperature of long aluminum alloy profiles, resulting in unstable mechanical properties, low production efficiency, high labor intensity, periodic changes in the environment, and unstable product quality.

Method used

A roll-bottom continuous solution heat treatment equipment for long aluminum alloy profiles is designed, including pre-furnace feed rollers, roll-bottom furnace gas circulation heating furnace, thermal insulation transition tunnel, multi-media graded cooling quencher, wet exhaust drying device and The discharge rollers use a multi-media hierarchical cooling quencher and an automated wet-drying drying device to achieve continuous production by controlling the temperature and time.

Benefits of technology

Effectively control temperature and time, improve product performance and quality, reduce production costs, improve production efficiency, avoid distortion and deformation caused by uneven temperature rise and cold speed of profiles during heating and quenching, and improve labor intensity and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110894571B_ABST
    Figure CN110894571B_ABST
Patent Text Reader

Abstract

The invention relates to a roller bottom continuous solid solution heat treatment equipment for aluminum alloy long profiles and a process thereof. The treatment equipment comprises a furnace front feeding roller table, a roller bottom furnace gas circulation heating furnace, a heat preservation transition tunnel, a multi-medium graded cooling quenching machine, a dehumidification drying device and a material discharge roller table which are sequentially connected end to end. The process comprises heating, heat preservation, quenching cooling, dehumidification drying and material discharge steps. The beneficial effects of the invention are as follows: the temperature remains unchanged during the solid solution heat treatment process, the soaking time is guaranteed, the alloy components of the material are fully diffused and homogenized, and the mechanical properties of the product are enhanced; the multi-medium graded cooling quenching machine reduces the distortion and deformation of the aluminum alloy long profiles during the cooling process, and improves the production capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid solution heat treatment, and in particular relates to a roller bottom type continuous solid solution heat treatment equipment suitable for long aluminum alloy profiles and a process thereof. Background Art

[0002] The traditional solution heat treatment process generally adopts "extrusion waste heat online solution heat treatment process", "well-type heating furnace + quenching tank solution process", and "box-type heating furnace + quenching tank solution process". The "extrusion waste heat online solution heat treatment process" has the disadvantages of uncontrollable initial quenching temperature, no temperature equalization process, and the product mechanical properties fluctuate; "well-type heating furnace + quenching tank solution process" and "box-type heating furnace + quenching tank solution process" work intermittently, and have the problems of low production capacity, high labor intensity, periodic changes in the heat treatment process environment, and unstable product quality. For this reason, we need a new type of roller bottom continuous solution heat treatment equipment and process suitable for aluminum alloy long profiles. Summary of the invention

[0003] The problem to be solved by the present invention is to provide a roller bottom continuous solution heat treatment equipment and process for aluminum alloy long profiles, which can control temperature and time, has high production efficiency, high product performance and quality, and low comprehensive investment.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a roller-bottom continuous solution heat treatment equipment for long aluminum alloy profiles, characterized in that it includes a pre-furnace feeding roller, a roller-bottom furnace gas circulation heating furnace, an insulation transition tunnel, a multi-medium graded cooling quenching machine, a dehumidification and drying device, a feeding roller and a conveying roller for conveying profiles arranged in sequence.

[0005] Furthermore, the heat-insulating transition tunnel comprises a shell, the inner wall of the shell is provided with heat-insulating material, the outer side of the shell is provided with a motor and a sprocket chain, and the motor drives the conveying roller to move through the sprocket chain.

[0006] Furthermore, the dehumidification and drying device includes a bracket and a roller-bottom transmission mechanism arranged at the bottom of the bracket, and a plurality of axial fans are evenly arranged at the top and bottom of the bracket. A lifting mechanism that can move up and down relative to the profile is also arranged in the bracket, and a plurality of air spray devices are arranged on the lifting mechanism.

[0007] Furthermore, the unloading roller includes a transmission roller at the end of the heat treatment production line and a discharge platform arranged on the side of the transmission roller, and also includes a conveying mechanism, which is controlled by a driving mechanism and performs lifting and / or transverse reciprocating motion between the transmission roller and the discharge platform.

[0008] A process for roller bottom continuous solution heat treatment equipment for long aluminum alloy sections, characterized in that it comprises the following steps:

[0009] (1) The aluminum alloy long profiles are heated in a roller hearth gas circulation heating furnace at a temperature of 450-550°C for 2-4 hours;

[0010] (2) After heating, the profile is driven by the conveyor roller to pass through the insulation transition tunnel, where the insulation temperature is 450-550°C;

[0011] (3) After passing through the insulation transition tunnel, the profile is driven by the conveyor roller and enters the multi-medium graded cooling quenching machine for quenching cooling. The quenching cooling rate is 100-400°C / min, the quenching air pressure is 5-15kPa, the quenching water pressure is 0.4-0.8MPa, the quenching water temperature is 30-60°C, and the speed of the profile passing through the quenching machine is 5-100m / min;

[0012] (4) After quenching and cooling, the profile is sent to the dehumidification drying device by the conveyor roller to remove the residual moisture on the inner and outer surfaces. The water blowing pressure is 10-15 kPa, the air drying pressure is 200-500 Pa, and the drying time is 1-3 minutes;

[0013] (5) After being dehumidified and dried, the profile is conveyed to the conveyor roller. The profile is moved horizontally to the unloading platform by the conveying mechanism, and the conveyor roller is vacant and waiting.

[0014] Furthermore, the profile is placed on an anti-scratch tray and enters the processing equipment.

[0015] The advantages and positive effects of the present invention are:

[0016] (1) The setting of the insulation transition tunnel avoids the multi-medium graded cooling quenching machine and the roller hearth gas circulation heating furnace from being too close, reduces the temperature impact of the multi-medium graded cooling quenching machine on the roller hearth gas circulation heating furnace, and avoids the cooling of the profile before entering the multi-medium graded cooling quenching machine, effectively ensuring the realization of the solid solution quenching process;

[0017] (2) The multi-medium graded cooling quenching machine can mix or superimpose different forms of quenching media (liquid, gas or gas + liquid) according to the cross-sectional characteristics of the profile, which greatly reduces the serious distortion and deformation of the long aluminum alloy profile caused by uneven temperature rise during heating and uneven cooling rate during quenching;

[0018] (3) The dehumidification and drying device can blow away the water on the surface of the profile, and the lifting mechanism can automatically move up and down to adjust the distance between the air spray device and the profile, thereby improving the dehumidification efficiency, reducing the collision between the air spray device and the profile and damaging the air spray device, and saving costs.

[0019] (4) The conveying mechanism keeps the unloading roller working continuously through the transverse reciprocating motion, thereby improving production capacity and labor intensity; BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram of the overall structure of an embodiment of the present invention

[0021] Figure 2 Schematic diagram of a dehumidification and drying device according to an embodiment of the present invention

[0022] Figure 3 The overall schematic diagram of the unloading roller conveyor with automatic lateral movement mechanism according to the embodiment of the present invention is

[0023] Figure 4 Schematic diagram of the structure of the unloading roller with automatic lateral movement mechanism according to the embodiment of the present invention

[0024] In the figure: 1. Front feeding roller table 2. Roller-type furnace gas circulation heating furnace 3. Multi-media graded cooling quenching machine 4. Dehumidification and drying device 5. Unloading roller table 6. Lifting mechanism 7. Air injection device 8. Axial flow fan 9. Conveying mechanism 10. Fixed beam group 11. Conveying roller table 12. Insulated transition tunnel 13. Unloading platform 14. Driving mechanism DETAILED DESCRIPTION

[0025] The following is a further description of an embodiment of the present invention in conjunction with the accompanying drawings: A roller-bottom continuous solution heat treatment equipment for long aluminum alloy profiles, comprising a front-furnace feeding roller 1, a roller-bottom furnace gas circulation heating furnace 2, an insulation transition tunnel 12, a multi-medium graded cooling and quenching machine 3, a dehumidification and drying device 4 and a discharge roller 5, which are connected in sequence, and also includes a conveying roller for conveying profiles.

[0026] The above-mentioned heat preservation transition tunnel 12 includes a shell, the inner wall of the shell is provided with heat insulation material, and the outer side of the shell is provided with a motor, and the motor drives the conveying roller to move by driving the sprocket chain. The setting of the heat preservation transition tunnel 12 not only avoids the multi-medium graded cooling quenching machine 3 from affecting the temperature in the roller hearth furnace gas circulation heating furnace 2, but also avoids the cooling of the profile before entering the multi-medium graded cooling quenching machine 3, and effectively ensures the realization of the solid solution quenching process.

[0027] The dehumidification and drying device 4 comprises a bracket and a roller bottom transmission mechanism arranged at the bottom of the bracket. A plurality of axial flow fans 8 are evenly arranged at the top and bottom of the bracket. A lifting mechanism 6 is also arranged in the bracket for moving up and down relative to the profile. A plurality of air jet devices 7 are arranged on the lifting mechanism 6. The lifting mechanism 6 adjusts the distance between the air jet device 7 and the profile according to the height of the profile. The air jet device 7 is arranged in the front position of the dehumidification and drying device 4 close to the multi-media graded cooling and quenching machine 3. The axial flow fan 8 is arranged in the rear position of the dehumidification and drying device 4 away from the multi-media graded cooling and quenching machine 3. When the profile passes through the dehumidification and drying device 4, the accumulated water remaining on the upper surface of the profile is first blown away by the air jet device 7, and then the evenly distributed plurality of axial flow fans 8 blow dry the attached water from the upper and lower surfaces of the profile respectively. The dehumidification and drying device 4 is an independent single unit device, and the outer shell structure is connected to the ground. The roller surface elevation of its roller bottom transmission mechanism is kept consistent with the front and rear devices, and the transmission speed is kept consistent with the adjacent sections during production.

[0028] The unloading roller 5 includes a conveying roller 11, a fixed beam group 10 and a conveying mechanism 9. The fixed beam group 10 is the integral steel structure of the unloading roller 5. The conveying mechanism 9 is controlled by a driving mechanism 14 to lift and / or reciprocate. The unloading roller 5 has two material levels (the conveying roller 11 at the end of the heat treatment production line and the unloading platform 13 on its side). After the profile is conveyed to the conveying roller 11, the conveying mechanism 9 rises, lifts the profile to separate from the conveying roller 11, and then maintains a high position and moves laterally to above the unloading platform 13 on the side. After that, the conveying mechanism 9 descends and places the profile on the unloading platform 13. Finally, the conveying mechanism 9 moves laterally from the low position back to below the conveying roller 11.

[0029] A process for a roller bottom type continuous solution heat treatment equipment for aluminum alloy long profiles comprises the following steps:

[0030] (1) Heating: Aluminum alloy long profiles are loaded on the anti-scratch tray and enter the roller hearth furnace gas circulation for heating. The anti-scratch tray moves forward continuously or rhythmically (the anti-scratch tray is fixedly heated on a material table for a period of time, and then moves a distance to the next material table for fixed heating) and completes the heating process. The heating temperature is 450-550°C, and the insulation time is 2-4 hours;

[0031] (2) Insulation: After heating, the profile is driven by the conveyor roller to pass through the insulation transition tunnel, where the insulation temperature is 450-550°C;

[0032] (3) Quenching and cooling: After the profile passes through the insulation transition tunnel, it is driven by the conveyor roller and enters the multi-medium graded cooling quenching machine for quenching and cooling. The quenching cooling rate is 100-400°C / min, the quenching air pressure is 5-15kPa, the quenching water pressure is 0.4-0.8MPa, the quenching water temperature is 30-60°C, and the speed of the profile passing through the quenching machine is 5-100m / min;

[0033] (4) Dehumidification: After quenching and cooling, the profile is sent to the dehumidification drying device by the conveyor roller to remove the residual moisture on the inner and outer surfaces. The water blowing pressure is 10-15 kPa, the air drying pressure is 200-500 Pa, and the drying time is 1-3 minutes;

[0034] (5) Unloading: After being dehumidified and dried, the profile is conveyed to the conveyor roller. The profile is moved horizontally to the unloading platform by the conveying mechanism, and the conveyor roller is empty and waiting.

[0035] In the embodiment of the present invention, the anti-scratch material tray is made of a heat-resistant alloy with a temperature resistance of more than 550°C, and the bearing surface is covered with an anti-scratch cushion layer with a temperature resistance of more than 550°C and resistant to wind / water erosion. The anti-scratch material tray adopts a lightweight design, which not only ensures the strength for repeated use, but also minimizes the weight and the consumption of energy media during the heat treatment process.

[0036] The present invention is further described in the following embodiments:

[0037] Embodiment 1: After the aluminum profiles of 4.2 series specifications complete the heating and heat preservation process, the quenching temperature is 495-520C during quenching cooling; the quenching air pressure is 10-15kPa; the water pressure is 0.4-0.5MPa, and then the dehumidification, drying and unloading process is completed.

[0038] Embodiment 2: After the 6 series aluminum profiles complete the heating and heat preservation process, the quenching temperature is 515-530C during quenching cooling; the quenching air pressure is 10-15kPa; the water pressure is 0.4-0.5MPa, and then the dehumidification, drying and unloading process is completed.

[0039] Embodiment 3: After the 7 series aluminum profiles complete the heating and heat preservation process, the quenching temperature is 460-485°C during quenching cooling; the quenching air pressure is 10-15 kPa; the water pressure is 0.4-0.5 MPa, and then the dehumidification, drying and unloading process is completed.

[0040] The advantages and positive effects of the present invention are:

[0041] (1) The setting of the insulation transition tunnel avoids the multi-medium graded cooling quenching machine and the roller hearth gas circulation heating furnace from being too close, reduces the temperature impact of the multi-medium graded cooling quenching machine on the roller hearth gas circulation heating furnace, and avoids the cooling of the profile before entering the multi-medium graded cooling quenching machine, effectively ensuring the realization of the solid solution quenching process;

[0042] (2) The multi-medium graded cooling quenching machine can mix or superimpose different forms of quenching media (liquid, gas or gas + liquid) according to the cross-sectional characteristics of the profile, which greatly reduces the serious distortion and deformation of the long aluminum alloy profile caused by uneven temperature rise during heating and uneven cooling rate during quenching;

[0043] (3) The dehumidification and drying device can blow away the water on the surface of the profile, and the lifting mechanism can automatically move up and down to adjust the distance between the air spray device and the profile, thereby improving the dehumidification efficiency, reducing the collision between the air spray device and the profile and damaging the air spray device, and saving costs.

[0044] (4) The conveying mechanism keeps the unloading roller working continuously through the transverse reciprocating motion, thereby improving production capacity and labor intensity;

[0045] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A roller-bottom continuous solution heat treatment equipment for long aluminum alloy profiles, characterized in that: It includes a furnace front feeding roller, a roller bottom furnace gas circulation heating furnace, a heat preservation transition tunnel, a multi-media graded cooling quenching machine, a dehumidification and drying device, a feeding roller and a conveying roller for conveying profiles arranged in sequence; the heat preservation transition tunnel includes a shell, the inner wall of which is provided with heat insulation material. A motor and a sprocket chain are disposed outside the housing, and the motor drives the conveying roller to move through the sprocket chain; The dehumidification and drying device comprises a bracket and a roller bottom transmission mechanism arranged at the bottom of the bracket, a plurality of axial flow fans are evenly arranged at the top and bottom of the bracket, a lifting mechanism that can move up and down relative to the profile is also arranged in the bracket, and a plurality of air spray devices are arranged on the lifting mechanism; The lifting mechanism adjusts the distance between the air spray device and the profile according to the profile height; the air spray device is arranged in the front position of the dehumidification and drying device close to the multi-media graded cooling and quenching machine, and the axial flow fan is arranged in the rear position of the dehumidification and drying device away from the multi-media graded cooling and quenching machine; The unloading roller includes a transmission roller at the end of the heat treatment production line and a discharge platform arranged on the side of the transmission roller, and also includes a conveying mechanism, which is controlled by a driving mechanism and performs lifting and / or transverse reciprocating motion between the transmission roller and the discharge platform.

2. A process for the roller-bottom continuous solution heat treatment equipment for aluminum alloy long profiles as claimed in claim 1, characterized in that: The steps include: (1) The aluminum alloy long profile enters a roller hearth gas circulation heating furnace for heating at a temperature of 450-550°C for 2-4 hours; (2) After heating, the profile is driven by the conveyor roller to pass through the insulation transition tunnel, where the insulation temperature is 450-550°C; (3) After passing through the insulation transition tunnel, the profile is driven by the conveyor roller and enters the multi-medium graded cooling quenching machine for quenching cooling. The quenching cooling rate is 100-400°C / min, the quenching air pressure is 5-15kPa, the quenching water pressure is 0.4-0.8MPa, the quenching water temperature is 30-60°C, and the speed of the profile passing through the quenching machine is 5-100m / min; (4) After quenching and cooling, the profile is sent to the dehumidification drying device by the conveyor roller to remove the residual moisture on the inner and outer surfaces. The water blowing pressure is 10-15 kPa, the air drying pressure is 200-500 Pa, and the drying time is 1-3 minutes; (5) After being dehumidified and dried, the profile is conveyed to the conveyor roller. The profile is moved horizontally to the unloading platform by the conveying mechanism, and the conveyor roller is empty and waiting.