A low surface energy nickel-chromium heating wire, preparation method and use thereof

By preparing a low-surface energy layer on the surface of the nickel-chromium heating wire, the combination of sol gel and low-surface energy layer is used to solve the problem of adhesion between e-liquid and carbon deposits, the heat conduction efficiency and user experience are improved, and the service life is extended.

CN111165904BActive Publication Date: 2024-11-15CHINA TOBACCO YUNNAN IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010015605.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-07
Publication Date
2024-11-15
Estimated Expiration
2040-01-07

AI Technical Summary

Technical Problem

Nickel-chromium heating wires are prone to cross-linking and gelatinization of e-liquid components due to high temperatures in electronic cigarettes, forming carbon deposits, affecting heat conduction efficiency and user experience, and the prior art has failed to effectively reduce the adhesion of e-liquid and carbon deposits.

Method used

The low-surface energy layer is prepared on the surface of the nickel-chromium heating wire. By combining sol gel and low-surface energy layer, the adhesion of e-liquid and carbon deposits is reduced by utilizing its micro-nano structure and low-surface energy characteristics.

Benefits of technology

It significantly reduces the adhesion of e-liquid and carbon deposits, improves the heat conduction efficiency and user experience of heating wires, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111165904B_ABST
    Figure CN111165904B_ABST
Patent Text Reader

Abstract

The invention discloses a low surface energy nickel-chromium heating wire, which comprises a sol-gel layer on the surface of the nickel-chromium wire and a low surface energy layer on the surface of the sol-gel layer. The invention also discloses a preparation method of the nickel-chromium heating wire and its use in reducing the adhesion of tobacco oil in electronic cigarettes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic cigarette materials, and in particular relates to a nickel-chromium heating wire with a low surface energy layer and low smoke oil adhesion and a preparation method thereof. Technical Background

[0002] As people's understanding of the harmful substances produced by traditional tobacco in the combustion process continues to deepen, new tobacco such as electronic cigarettes are constantly being developed and have achieved rapid development. Compared with traditional cigarettes, the characteristics of electronic cigarettes are that the electronic cigarette liquid is refined, does not produce toxic smoke, does not contain carbon monoxide that is harmful to the human body, and it is heated and turned into steam, part of which enters the human lungs, and the other part is exhaled into the air. The particles and tar in the smoke do not contain carcinogens;

[0003] Electronic cigarette oil, also known as electronic cigarette liquid, is an electronic atomizing liquid used with electronic cigarettes. It can produce cigarette-like mist by heating it in the electronic cigarette atomizer, generally 0.5 to 1 ml is required at a time. The main components of the oil are glycerin, propylene glycol, plant flavors, nicotine, etc. Nicotine is added to the electronic cigarette oil mainly to make it taste closer to cigarettes. When using, pay attention to the amount of oil in the atomizer. Too little oil will cause damage to the atomizer and a burnt taste.

[0004] The role of flavors in e-liquid is very important. The flavor of e-liquid is determined by the flavors. The combination of different flavors and flavors determines the flavor of a e-liquid. Fragrance raw materials are divided into artificial synthetic fragrance raw materials and natural extract flavors. The U.S. Food and Drug Administration defines "natural fragrance raw materials" as oils, resins or other extracts from natural sources such as plants, meat or seafood. In the process of extracting flavors, processing processes such as heating or fermentation are used. The function of the resulting product is only to flavor, not to add any nutrients. Basically, if something is a natural fragrance raw material, it is a derivative of a natural resource. Some consumers prefer to use natural fragrance raw materials rather than artificial fragrance raw materials because they believe that products containing natural fragrance raw materials may be healthier. However, considering factors such as purification costs and technology, the extracts of natural flavors will contain more complex components, such as sugars, some of which will undergo thermal decomposition at high temperatures, making it easier for e-liquid to adhere to and decompose on the heating element.

[0005] As one of the commonly used electronic cigarette heating wire materials, during the heating process of nickel-chromium heating wire, some components in the electronic cigarette liquid will undergo cross-linking and gelatinization under the action of high temperature to form carbon deposits. These gelatinized products adhere to the surface of the heating wire, which will affect the heat conduction efficiency of the heating wire on the one hand, and on the other hand, the gelatinized products will produce a special odor, affecting the user's sensory experience.

[0006] At present, the surface of the nickel-chromium heating wire used in electronic cigarettes is mostly not treated and is used directly, and there is no relevant report on reducing the adhesion of tobacco oil and carbon deposits on the nickel-chromium heating wire used in electronic cigarettes. The present invention prepares a coating capable of repelling electronic cigarette oil on the surface of the nickel-chromium heating wire, and utilizes the surface's repelling effect on electronic cigarette oil to achieve the effect of reducing the adhesion of electronic cigarette oil and carbon deposits on the nickel-chromium heating wire. Summary of the invention

[0007] Aiming at the problem that the tobacco oil in most nickel-chromium wires used in electronic cigarettes is easily gelatinized during operation, the present invention provides a nickel-chromium heating wire with a low surface energy layer having a low tobacco oil adhesion effect and a preparation method thereof.

[0008] The technical solution of the present invention is as follows:

[0009] A first aspect of the present invention provides a nickel-chromium heating wire, which comprises a sol-gel layer on the surface of the nickel-chromium wire and a low surface energy layer on the surface of the sol-gel layer.

[0010] Preferably, the contact angle of the tobacco oil to the nickel-chromium heating wire is greater than 150° and the amount of tobacco oil adhered to the surface of the nickel-chromium heating wire is less than 5wt%.

[0011] Preferably, the nickel-chromium heating wire material is a nickel-chromium alloy, and its resistance is 0.1-2Ω.

[0012] Preferably, the sol-gel layer has a micro-nano structure.

[0013] Preferably, the low surface energy layer is a layer formed of a silicon compound, a fluorine compound or a mixture of the two.

[0014] The second aspect of the present invention discloses a method for preparing the nickel-chromium heating wire, comprising the following steps:

[0015] ① Mix the solvent, ammonia water, film-forming components and deionized water for 1 to 48 hours and then age them for 1 to 14 days to obtain a sol-gel solution;

[0016] ② Mix the solvent, glacial acetic acid, HCl, low surface energy components and deionized water for 1 to 48 hours and then age them for 1 to 14 days to obtain a low surface energy solution;

[0017] ③ Apply the sol-gel solution obtained in step ① to the surface of the nickel-chromium heating wire, put it in an oven at 60-120°C, and treat it for 0.5-2h to obtain a sol-gel treated nickel-chromium heating wire. ;

[0018] ④ Apply the low surface energy solution obtained in step ② to the surface of the nickel-chromium wire with the sol-gel layer obtained in step ③, dry it at 120-220° C. for 1-6 hours, and then obtain the nickel-chromium heating wire.

[0019] Preferably, the mass ratio of each substance in the sol-gel solution of step ① is: solvent 70-95, ammonia water 0.1-5, film-forming component 0.5-20, deionized water 0.1-10; the solvent is ethanol, or a mixture of ethanol and one or more of methanol, ethanol, isopropanol, n-butanol, n-hexanol, ethylene glycol, ethylene glycol methyl ether, ethylene glycol monomethyl ether, propylene glycol or propylene glycol dimethyl ether; the film-forming component is one or more of tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, and n-butyl titanate.

[0020] Preferably, the mass ratio of each substance in the low surface energy solution in step ② is: solvent 70-95, glacial acetic acid 0.1-5, HCl (0.01M) 1-5, low surface energy component 0.5-20, deionized water 0.1-10; the solvent is ethanol, or a mixture of ethanol and one or more of methanol, ethanol, isopropanol, n-butanol, n-hexanol, ethylene glycol, ethylene glycol methyl ether, ethylene glycol monomethyl ether, propylene glycol or propylene glycol dimethyl ether; the low surface energy component is tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trifluoropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropylmethyldimethoxysilane, perfluorodecyltrimethoxysilane, perfluorodecyltriethoxysilane, perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane. One or more of silane.

[0021] Preferably, the low surface energy solution in step ② also contains a flexibilizer in a mass ratio of 0.1 to 5 and a coupling agent in a mass ratio of 0.1 to 2; the flexibilizer is one or more of dimethyldimethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane or trimethylethoxysilane; the coupling agent is one of KH550 or KH560, wherein KH550 is γ-aminopropyltriethoxysilane and KH560 is γ-glycidyloxypropyltrimethoxysilane.

[0022] Preferably, before coating the surface of the nickel-chromium wire with the sol-gel solution in step ③, the nickel-chromium wire is ultrasonically cleaned with acetone, ethanol and deionized water in sequence, and air-dried with nitrogen.

[0023] The third aspect of the present invention discloses the use of the nickel-chromium heating wire for low-liquid adhesion electronic cigarettes.

[0024] Beneficial effects of the present invention:

[0025] 1. The surface energy of the nickel-chromium heating wire of the present invention is low, which can significantly reduce the adhesion of tobacco oil. After being used for a period of time, the surface carbon content of the nickel-chromium heating wire of the present invention is very small, which can meet the needs of heating the tobacco oil of electronic cigarettes.

[0026] 2. The surface of the nickel-chromium heating wire of the present invention has a sol-gel layer and a micro-nano structure, which not only enhances the bonding force between the low surface energy layer and the base nickel-chromium wire, but also significantly reduces the surface energy of the low surface energy layer. The adhesion amount and carbon deposition amount of the electronic cigarette oil can be significantly reduced; while the low surface energy layer is directly coated on the surface of the nickel-chromium wire, the surface energy of the nickel-chromium heating wire is not significantly reduced, and the adhesion amount and carbon deposition amount of the cigarette oil are relatively large.

[0027] 3. The preparation steps of the sol-gel layer and the low surface energy layer of the present invention are simple, and the sol-gel solution and the low surface energy solution can be applied to the surface of the sol-gel nickel-chromium wire by spraying or dipping. The preparation method of the present invention is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the surface morphology of nickel-chromium wire after sol-gel. DETAILED DESCRIPTION

[0029] Example 1

[0030] Preparation of sol-gel solution: Add 30 ml of ethanol, 0.2 ml of ammonia water, 2 ml of n-hexanol, and 5 ml of methyltriethoxysilane in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.2 g of deionized water, stir for 24 hours, and age at room temperature for 2 days to obtain an apparently uniform sol-gel solution.

[0031] Preparation of low surface energy solution: Add 30 ml of ethanol, 0.9 ml of glacial acetic acid, 2 ml of n-hexanol, 0.1 ml of HCl (0.01M), 5 ml of methyltriethoxysilane, and 0.5 ml of KH550 in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.2 g of deionized water, stir for 24 hours, and age at room temperature for 7 days to obtain an apparently uniform sol-gel solution.

[0032] The obtained sol-gel solution was diluted 100 times with anhydrous ethanol.

[0033] The obtained low surface energy solution was diluted 100 times with anhydrous ethanol.

[0034] The nickel-chromium wire was ultrasonically cleaned with acetone, ethanol and deionized water in turn, and air-dried with nitrogen. The nickel-chromium wire was then dip-coated in a sol-gel solution, dried at room temperature, and then treated in an oven at 60°C for 0.5h to obtain the sol-gel treated nickel-chromium wire. Figure 1 As shown, there is a micro-nanopore structure thereon.

[0035] The nickel-chromium wire treated with the sol-gel is placed in a low surface energy solution for dip coating, dried at room temperature, and then treated in an oven at 220° C. for 6 hours to obtain the nickel-chromium heating wire.

[0036] The obtained nickel-chromium heating wire was evaluated with commonly used electronic cigarette oil and the results are as follows:

[0037]

[0038] [Note] The nickel-chromium substrate used in the contact angle test is a nickel-chromium sheet. The nickel-chromium substrate + low surface energy layer is a nickel-chromium substrate directly coated with a low surface energy solution without sol-gel. The nickel-chromium substrate used in the smoke oil adhesion test is a nickel-chromium wire. The steps are to immerse the sample in the smoke oil for one minute and take it out, weigh the mass of the sample before and after immersion in the smoke oil, and the extra mass of the sample after immersion in the smoke oil accounts for the percentage of the sample mass.

[0039] From the data in the table, it can be seen that sample 3 with a sol-gel layer can significantly reduce the adhesion of smoke oil. After the sample was electrified in the smoke oil 10 times (temperature 188-500℃, each electrification for 5 minutes), the carbon deposit on the surface of sample 3 was only 0.5wt%; pure nickel-chromium was 5.3wt%, and the nickel-chromium wire of the sample without a sol-gel layer was 4.6wt%, see the last column of data in the above table. This may be because the sol-gel layer has a micro-nano pore structure, which not only enhances the bonding force between the low surface energy layer and the base nickel-chromium wire, but also significantly reduces the surface energy of the low surface energy layer; after electrification 10 times, the bonding force of the low surface energy layer is still strong and the structure of the low surface energy layer changes little.

[0040] Example 2

[0041] Preparation of sol-gel solution: Add 30 ml of ethanol, 0.5 ml of ammonia water, 2 ml of n-hexanol, and 5 ml of methyltriethoxysilane in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 1 g of deionized water, stir for 12 h, and age at room temperature for 7 days to obtain an apparently uniform sol-gel solution.

[0042] Preparation of low surface energy solution: In a three-necked flask, add 30 ml of ethanol, 0.3 ml of glacial acetic acid, 12 ml of n-hexanol, 0.5 ml of HCl (0.01 M), 5 ml of methyltriethoxysilane, 0.5 ml of perfluorodecyltriethoxysilane, and 0.5 ml of KH550 in sequence, stir and mix evenly at room temperature, then add 0.4 g of deionized water, stir for 12 h, and age at room temperature for 5 days to obtain an apparently uniform sol-gel solution.

[0043] The obtained sol-gel solution was diluted 100 times with anhydrous ethanol.

[0044] The obtained low surface energy solution was diluted 100 times with anhydrous ethanol.

[0045] The nickel-chromium wire was ultrasonically cleaned with acetone, ethanol and deionized water in sequence, and air-dried with nitrogen. The nickel-chromium wire was then dip-coated in a sol-gel solution, dried at room temperature, and then treated in an oven at 120° C. for 2 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0046] The sol-gel treated nickel-chromium wire is placed in a low surface energy solution for dip coating, dried at room temperature, and then treated in an oven at 120° C. for 6 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0047] The test results are similar to those of Example 1.

[0048] Example 3

[0049] Preparation of sol-gel solution: Add 30 ml of ethanol, 0.3 ml of ammonia water, 2 ml of n-hexanol, 5 ml of methyltriethoxysilane, and 2 ml of n-butyl titanate in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.6 g of deionized water, stir for 2 h, and age at room temperature for 7 days to obtain an apparently uniform sol-gel solution.

[0050] Preparation of low surface energy solution: Add 30 ml of ethanol, 0.3 ml of glacial acetic acid, 12 ml of n-hexanol, 2 ml of HCl (0.01 M), 5 ml of methyltriethoxysilane, 2 ml of perfluorooctyltriethoxysilane, and 0.5 ml of KH550 in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.5 g of deionized water, stir for 12 h, and age at room temperature for 5 days to obtain an apparently uniform sol-gel solution.

[0051] The obtained sol-gel solution was diluted 100 times with anhydrous ethanol.

[0052] The obtained low surface energy solution was diluted 100 times with anhydrous ethanol.

[0053] The nickel-chromium wire was ultrasonically cleaned with acetone, ethanol and deionized water in sequence, and air-dried with nitrogen. The nickel-chromium wire was then dip-coated in a sol-gel solution, dried at room temperature, and then treated in an oven at 120° C. for 6 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0054] The sol-gel treated nickel-chromium wire is placed in a low surface energy solution for dip coating, dried at room temperature, and then treated in an oven at 150° C. for 3 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0055] The test results are similar to those of Example 1.

[0056] Example 4

[0057] Preparation of sol-gel solution: Add 30 ml of ethanol, 0.2 ml of ammonia water, 2 ml of n-hexanol, and 5 ml of tetraethoxysilane in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.5 g of deionized water, stir for 2 h, and age at room temperature for 7 days to obtain an apparently uniform sol-gel solution.

[0058] Preparation of low surface energy solution: Add 30 ml of ethanol, 0.3 ml of glacial acetic acid, 12 ml of n-hexanol, 2 ml of HCl (0.01 M), 5 ml of methyltriethoxysilane, 1 ml of perfluorooctyltriethoxysilane, and 0.5 ml of KH550 in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.4 g of deionized water, stir for 12 h, and age at room temperature for 5 days to obtain an apparently uniform sol-gel solution.

[0059] The obtained sol-gel solution was diluted 100 times with anhydrous ethanol.

[0060] The obtained low surface energy solution was diluted 100 times with anhydrous ethanol.

[0061] The nickel-chromium wire was ultrasonically cleaned with acetone, ethanol and deionized water in sequence, and air-dried with nitrogen. The nickel-chromium wire was then dip-coated in a sol-gel solution, dried at room temperature, and then treated in an oven at 120° C. for 2 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0062] The sol-gel treated nickel-chromium wire is placed in a low surface energy solution for dip coating, dried at room temperature, and then treated in an oven at 220° C. for 6 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0063] The test results are similar to those of Example 1.

[0064] Example 5

[0065] Preparation of sol-gel solution: Add 30 ml of ethanol, 0.5 ml of ammonia water, 2 ml of n-hexanol, and 5 ml of tetramethoxysilane in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.5 g of deionized water, stir for 1 hour, and age at room temperature for 7 days to obtain an apparently uniform sol-gel solution.

[0066] Preparation of low surface energy solution: Add 30 ml of ethanol, 0.3 ml of glacial acetic acid, 12 ml of n-hexanol, 2 ml of HCl (0.01 M), 5 ml of methyltriethoxysilane, 0.2 ml of trifluoropropylmethyldimethoxysilane, and 0.5 ml of KH560 in a three-necked flask in sequence, stir and mix evenly at room temperature, then add 0.4 g of deionized water, stir for 12 h, and age at room temperature for 5 days to obtain an apparently uniform sol-gel solution.

[0067] The obtained sol-gel solution was diluted 100 times with anhydrous ethanol.

[0068] The obtained low surface energy solution was diluted 100 times with anhydrous ethanol.

[0069] The nickel-chromium wire was ultrasonically cleaned with acetone, ethanol and deionized water in sequence, and air-dried with nitrogen. The nickel-chromium wire was then dip-coated in a sol-gel solution, dried at room temperature, and then treated in an oven at 120° C. for 2 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0070] The sol-gel treated nickel-chromium wire is placed in a low surface energy solution for dip coating, dried at room temperature, and then treated in an oven at 220° C. for 6 hours to obtain the sol-gel treated nickel-chromium heating wire.

[0071] The test results are similar to those of Example 1.

Claims

1. A nickel-chromium heating wire, characterized in that: It comprises a sol-gel layer on the surface of the nickel-chromium wire and a low surface energy layer on the surface of the sol-gel layer; the contact angle of the tobacco oil on the nickel-chromium heating wire is greater than 150° and the adhesion amount of the tobacco oil on the surface of the nickel-chromium heating wire is less than 5wt%; the sol-gel layer has a micro-nanopore structure; The low surface energy layer is a layer formed by a silicon compound, a fluorine compound or a mixture of the two; The preparation method of the nickel-chromium heating wire comprises the following steps: ① Mix the solvent, ammonia water, film-forming components and deionized water for 1 to 48 hours and then age them for 1 to 14 days to obtain a sol-gel solution; ② Mix the solvent, glacial acetic acid, hydrochloric acid, low surface energy components and deionized water for 1 to 48 hours and then age for 1 to 14 days to obtain a low surface energy solution; ③ Apply the sol-gel solution obtained in step ① to the surface of the nickel-chromium heating wire, and dry it at 60-120° C. for 0.5-2 h to obtain a sol-gel treated nickel-chromium heating wire; ④ Apply the low surface energy solution obtained in step ② to the surface of the nickel-chromium wire coated with the sol-gel layer obtained in step ③, and dry at 120-220° C. for 1-6 hours to obtain the nickel-chromium heating wire; Step ① The mass ratio of each substance in the sol-gel solution is: solvent 70-95, ammonia water 0.1-5, film-forming component 0.5-20, deionized water 0.1-10; the solvent is ethanol, or a mixture of ethanol and one or more of methanol, isopropanol, n-butanol, n-hexanol, ethylene glycol, ethylene glycol monomethyl ether, propylene glycol or propylene glycol dimethyl ether; the film-forming component is one or more of tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, and n-butyl titanate; Step ② The mass ratio of each substance in the low surface energy solution is: solvent 70-95, glacial acetic acid 0.1-5, 0.01M HCl 1-5, low surface energy component 0.5-20, deionized water 0.1-10; the solvent is ethanol, or a mixture of ethanol and one or more of methanol, isopropanol, n-butanol, n-hexanol, ethylene glycol, ethylene glycol monomethyl ether, propylene glycol or propylene glycol dimethyl ether; the low surface energy component is tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trifluoropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropylmethyldimethoxysilane, perfluorodecyltrimethoxysilane, perfluorodecyltriethoxysilane, perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane. One or more of silane.

2. The nickel-chromium heating wire according to claim 1, characterized in that: The nickel-chromium heating wire material is a nickel-chromium alloy, and its resistance is 0.1-2Ω.

3. The nickel-chromium heating wire according to claim 1, characterized in that: The sol-gel solution of step ① also contains a flexibilizer in a mass ratio of 0.1 to 5 and a coupling agent in a mass ratio of 0.1 to 2; the flexibilizer is one or more of dimethyldimethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane or trimethylethoxysilane; the coupling agent is one of KH550 or KH560.

4. The nickel-chromium heating wire according to claim 3, characterized in that: Before coating the surface of the nickel-chromium wire with the sol-gel solution in step ③, the nickel-chromium wire is ultrasonically cleaned with acetone, ethanol and deionized water in sequence, and air-dried with nitrogen.

5. Use of the nickel-chromium heating wire according to any one of claims 1 to 4 in reducing the adhesion of tobacco oil in electronic cigarettes.