Wind turbine blade root component production method and mold
Through the preformed blade matrix assembly and forming method, the problems of complex processing of wind power blade roots and difficult to ensure quality are solved, the production efficiency and infusion quality are improved, and the assembly process is simplified.
Patent Information
- Application Number
- CN201911370578.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-12-26
AI Technical Summary
The root processing of existing wind power blades is complex and difficult to guarantee. Especially under large loads, the overall infusion is difficult, time is long and lacks guarantee in the prior art.
The preformed upper and lower substrates are adopted, and the assembly and molding method in the mold is used to cure the assembly and form the assembly using adhesives to reduce the later overall filling steps, improve the filling quality, and reduce the assembly difficulty by stacking the blocks.
The production efficiency of wind power blade root assembly is improved, the perfusion quality is ensured, the defect rate is reduced, and the assembly process is simplified to meet the general needs of different models.
Smart Images

Figure CN111169041B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of wind power generation devices, and in particular to a method and a mould for producing a wind power blade root component. Background Art
[0002] Wind power generation is the fastest growing resource utilization method in the world today. As an important component of wind turbines, the development of wind turbine blades affects the development of the entire industry. With the expansion of the offshore market and the design of longer blades, the load on the root of the blades is becoming larger and larger, which places higher requirements on the production and processing of the root of wind turbine blades. In order to adapt to the problem of increasing blade root load, the main solutions are:
[0003] 1. Thickening the blade root layer. The increase in the thickness of the blade root layer will lead to a longer production layer operation time. The existing blade root thickness is generally more than 100mm. A greater thickness will further increase the difficulty of infusion and increase the infusion time.
[0004] 2. Design a larger pitch circle diameter. In the prior art, the semicircle height of the blade root pitch circle has exceeded the height of the operator, which makes its assembly and production difficult and brings great difficulty to the operator.
[0005] The Chinese patent application with publication number CN100402374C provides a blade root molding method, which sequentially places an outer shell layer, a previously manufactured support with a concave portion, a lower fiber pad, a screw sleeve, an upper fiber pad, a glass fiber tape, and a fiber pad, and then molds the blade root by vacuum infusion or the like. The disadvantage of the above-mentioned application method is that in order to reduce the weight of the entire blade root, an additional foam-molded support needs to be manufactured, and the installation steps of the upper and lower fiber pads and the glass fiber pad are relatively complicated, and the operation time is long. The overall solution adopts one-piece injection molding, and the infusion quality cannot be guaranteed. Summary of the invention
[0006] The object of the present invention is to provide a method and a mould for producing a wind turbine blade root assembly, so as to solve the technical problems in the prior art that the wind turbine blade root is complicated to process and the quality is difficult to ensure.
[0007] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for producing a wind turbine blade root assembly, comprising the following steps:
[0008] Preforming an upper substrate and a lower substrate, wherein the upper substrate and the lower substrate are both a single sheet of material, and the lower substrate is provided with a plurality of first grooves;
[0009] Placing the lower substrate in a mold, placing a plurality of embedded parts in the first groove, and buckling the upper substrate onto the embedded parts;
[0010] Adhesive is coated or laid on the lower substrate and the upper substrate respectively, and bonded to the embedded parts, or adhesive is filled between the lower substrate, the embedded parts and the upper substrate to form a composite part;
[0011] The assembly is cured in a mold.
[0012] Furthermore, the upper matrix and / or the lower matrix is a fiber-reinforced composite material.
[0013] Furthermore, the upper substrate and / or the lower substrate are formed by pultrusion.
[0014] Further, the lower substrate has a second fixed cross section, and the lower substrate is pultruded along the base line by the second fixed cross section;
[0015] The upper substrate has a first fixed cross-section, and the upper substrate is pultruded along a base line from the first fixed cross-section.
[0016] Further, the length directions of the first fixed cross section and the second fixed cross section are consistent with the length direction of the first groove, and the baseline is perpendicular to the first fixed cross section and the second fixed cross section.
[0017] Furthermore, the shape of the first fixed cross section and / or the second fixed cross section is a trapezoid.
[0018] Further, the length of the first fixed cross section is smaller than the length of the second fixed cross section.
[0019] Furthermore, after the embedded component is placed in the first groove, a filling component is arranged on one side of the embedded component, and at least a portion of the filling component is spliced with the embedded component and embedded in the first groove together.
[0020] Furthermore, the second fixing cross section includes a first portion corresponding to the embedded part and a second portion corresponding to the filling part in the first groove, and the first portion and the second portion have different thicknesses.
[0021] Furthermore, the sum of the length of the filling piece in the first groove and the length of the embedded piece is smaller than the length of the first groove.
[0022] Furthermore, a filling extension piece is provided between adjacent embedded parts (1).
[0023] Furthermore, a plurality of second grooves are provided on the upper substrate, and the first grooves and the second grooves are arranged opposite to each other and enclosed on the outside of the embedded part.
[0024] The present invention also discloses a mold, which is used in the production method of wind turbine blade root components, including a lower mold for accommodating the lower substrate and an upper mold for accommodating the upper substrate, and the lower mold is provided with a plurality of third grooves that fit with the lower surface of the lower substrate.
[0025] Furthermore, the upper mold is rotatably connected to the lower mold, and a plurality of fourth grooves that fit with the upper surface of the upper substrate are formed in the upper mold.
[0026] The beneficial effects of the wind turbine blade root assembly production method and mold provided by the present invention are as follows: compared with the prior art, the wind turbine blade root assembly production method and mold provided by the present invention preform the upper substrate and the lower substrate in advance, then place the upper substrate, the lower substrate and the embedded parts in the mold for assembly and molding, and then uniformly heat and cure, without the need for overall pouring during later processing, the pouring quality is higher, the difficulty and time of later pouring molding can be reduced, the defect rate can be reduced, and the overall height consistency can be ensured. The upper substrate and the lower substrate can be preformed separately, which can greatly save time and improve production efficiency, and the processed prefabricated parts can be stored and assembled in sections, using a block stacking method in the thickness direction and a multi-section prefabricated part splicing method in the circumferential direction, which can greatly reduce the difficulty of assembly. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 A schematic structural diagram of mold processing for a prefabricated component production method provided by an embodiment of the present invention;
[0029] Figure 2 A schematic diagram of the three-dimensional structure of a prefabricated part produced by the method for producing a prefabricated part of a wind turbine blade root provided by an embodiment of the present invention;
[0030] Figure 3 for Figure 2 Another perspective view of the preform shown, wherein the upper substrate is not shown;
[0031] Figure 4 for Figure 2 The main structure diagram of the prefabricated parts shown Figure 1 , the prefabricated parts are aligned and spliced;
[0032] Figure 5for Figure 2 The main structure diagram of the prefabricated parts shown Figure 2 , the prefabricated parts are spliced in a staggered manner;
[0033] Figure 6 A schematic diagram of the structure of the upper substrate and the lower substrate being extruded in the preform production method provided by an embodiment of the present invention;
[0034] Figure 7 A schematic diagram of the three-dimensional structure of a mold used in an embodiment of the present invention;
[0035] Figure 8 A schematic structural diagram of a blade root provided in an embodiment of the present invention.
[0036] Description of reference numerals:
[0037] 1. Embedded parts; 2. Lower substrate; 3. Upper substrate; 4. Adhesive layer; 5. Filling parts; 6. Mold; 7. Outer fiber fabric; 8. Inner fiber fabric; 21. First groove; 22. Inclined guide surface; 23. Second fixed section; 24. Base line; 31. Second groove; 32. Inclined surface; 33. First fixed section; 34. Base line; 51. Filling rod; 52. Filling ears; 61. Upper mold; 62. Lower mold; 611. Fourth groove; 621. Third groove; 6111. First groove section; 6112. Second groove section. DETAILED DESCRIPTION
[0038] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0040] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0041] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0042] Example 1
[0043] Please also read Figures 1 to 5 The wind turbine blade root prefabricated component production method provided by the present invention is now described. The wind turbine blade root prefabricated component production method comprises the following steps:
[0044] S1. Preforming an upper substrate 3 and a lower substrate 2, wherein the upper substrate 3 and the lower substrate 2 are both a single sheet of material, and the lower substrate 2 is provided with a plurality of first grooves 21;
[0045] S2. The lower substrate 2 is placed in the mold 6, and a plurality of embedded parts 1 are placed in the first groove 21, the upper substrate 3 is buckled on the embedded part 1, and the first groove 21 and the second groove 31 are arranged opposite to each other and enclosed on the outside of the embedded part 1;
[0046] S3. Adhesive is applied to the lower substrate 2 and the upper substrate 3 respectively, and they are bonded to the embedded part 1, so that the upper substrate 3, the embedded part 1 and the lower substrate 2 can be bonded into an assembly; wherein, the adhesive can be applied before the embedded part 1 is placed on the lower substrate 2, and a layer of adhesive is applied on the lower substrate 2, and when the upper substrate 3 is buckled on the embedded part 1, the adhesive is applied on the embedded part 1 or on the bottom of the upper substrate 3.
[0047] S4. The assembled components are solidified and molded in the mold 6 to form a preform.
[0048] Compared with the prior art, the method for producing the prefabricated root of a wind turbine blade provided by the present invention preforms the upper substrate 3 and the lower substrate 2 in advance, and then places the upper substrate 3, the lower substrate 2 and the embedded part 1 in a mold 6 for assembly and forming, and then uniformly heats and solidifies, without the need for overall pouring during later processing, and the pouring quality is higher, which can reduce the difficulty and time of later pouring and forming, reduce the defect rate, and ensure the overall height consistency. The upper substrate 3 and the lower substrate 2 can be preformed separately, which can greatly save time and improve production efficiency, and the processed prefabricated parts can be stored and assembled in sections, and the block stacking method is adopted in the thickness direction, and the multi-section prefabricated parts are spliced in the circumferential direction, which can greatly reduce the difficulty of assembly. At the same time, the prefabricated parts can be produced in a standardized and modular manner, can be made in advance, and defects can be easily checked and controlled, and risks can be reduced, which can further improve production efficiency, can achieve universal use of different models, and facilitate standardized management. At this time, the upper substrate 3 and the lower substrate 2 are both pre-processed and formed, and the bonding layer 4 is a later filler used to achieve a fixed connection between the upper substrate 3, the embedded part 1 and the lower substrate 2. The production method is simple and can be pre-produced. The single volume is small and the size of the entire prefabricated part can be adjusted according to demand. It is easy to check and control defects to reduce risks.
[0049] The structure of the prefabricated parts produced by the above-mentioned prefabricated parts production party is as follows: the prefabricated parts include embedded parts 1, a lower substrate 2, an upper substrate 3 and an adhesive layer 4, the lower substrate 2 is a single-piece body, and its adjacent two side edges are respectively arranged along the first direction and the second direction, the extension direction of several embedded parts 1 is the second direction, and the embedded parts 1 are arranged on the lower substrate 2 along the first direction, and a first groove 21 is formed on the lower substrate 2 that is engaged with the outer edge of the embedded part 1; the upper substrate 3 is a single-piece body, and the upper substrate 3 is covered on the embedded part 1; the adhesive layer 4 is filled between the lower substrate 2 and the upper substrate 3 and is arranged around the outer edge of the embedded part 1.
[0050] The embedded part 1 can be a nut, a bolt stopper, a foam filler, a wooden object, a spacer, a three-dimensional fiber structure, or other parts that need to be embedded in the blade root as it is formed. It can be understood that the embedded part 1 is a part that is pre-formed before assembly. At the same time, in order to facilitate assembly and improve the interface bonding strength, its surface will be treated accordingly, such as winding fibers or yarns, attaching a peelable layer, surface processing, coating with resin or adhesive. Specifically, the embedded part 1 refers to a bolt structure arranged at intervals along the circumference of the blade root, which is used to connect the blade to the hub of the wind turbine generator through bolts. The first direction and the second direction are two mutually perpendicular directions on the horizontal plane. The arrangement extension direction of the embedded part 1 is perpendicular to the length extension direction of the first groove 21, that is, a plurality of embedded parts 1 are evenly spaced and arranged on the lower substrate 2.
[0051] The upper substrate 3 may be formed with a second groove 31 that engages with the outer edge of the embedded part 1, and the first groove 21 and the second groove 31 are arranged opposite to each other. The first groove 21 is evenly arranged along the first direction of the lower substrate 2, and the length direction of the first groove 21 is consistent with the length direction of the lower substrate 2, both being the second direction; the second groove 31 is also evenly arranged along the first direction of the upper substrate 3, and the first groove 21 and the second groove 31 are oppositely arranged and enclosed as a through hole, and the embedded part 1 is embedded in the through hole. The first groove 21 and the second groove 31 may be formed by bending the sheet of the lower substrate 2 or the sheet of the upper substrate 3 to form a wavy sheet, or may be formed by directly opening grooves on the sheet of the lower substrate 2 or the sheet of the upper substrate 3. Of course, according to actual conditions and specific needs, in other embodiments of the present invention, the upper substrate 3 can also be directly fastened to the embedded part 1 without opening the second groove 31 on the upper substrate 3. At this time, the shape of the embedded part 1 may be semicircular or square, etc., which is not the only limitation here.
[0052] Specifically, the embedded part 1 refers to a bolt structure arranged at intervals along the circumferential direction of the blade root, which is used to achieve a fixed connection with the blade, and the cross-sectional shape of the embedded part 1 is generally a cylindrical ring body, which is directly processed using standard parts, and the embedded part 1 in the shape of an oblate cylinder, a square body or other polygonal cross-sections can also be used; the adhesive can be made of any material, and can be adhesive glue, resin or prepreg fiber, etc., and can also be other materials that can synthesize several sub-components into a whole, such as epoxy adhesive, etc.
[0053] The upper matrix 3 and / or the lower matrix 2 are preformed reinforced fiber components, which are formed by impregnating the fibers with resin and curing them, such as by using prepreg process, pultrusion process or continuous molding process. Among them, the fibers are mainly glass fiber, carbon fiber, natural fiber, polyester fiber, polyamide fiber, etc. or a combination thereof, and the resin can be any thermosetting resin or thermoplastic resin such as epoxy resin, phenolic resin, unsaturated polyester, thermosetting resin, polyolefin, polyester resin, polyamide resin, etc. Preferably, the upper matrix 3 and the lower matrix 2 are both pre-processed sheets, which are respectively covered on the upper and lower sides of the embedded part 1, and the material is preferably multi-axial fiber and thermosetting resin, and the surface of the upper matrix 3 and the lower matrix 2 needs to be laid with a demoulding cloth or other surface roughening methods to ensure the roughness, such as sandblasting, sanding, grinding, corona treatment, plasma treatment, etc.
[0054] Preferably, the cross-sectional shape of the embedded part 1 is circular or elliptical, and the first groove 21 and the second groove 31 are combined to form a circle or an ellipse. Specifically, the cross-sectional shape of the embedded part 1 is generally circular or elliptical, that is, the embedded part 1 is a circular cylinder, and the inner surface of the embedded part 1 is provided with an internal thread, and the bolt can be inserted into the through hole in the embedded part 1, thereby realizing the connection of the bolt. The first groove 21 and the second groove 31 are arranged opposite to each other, that is, the two first grooves 21 and the second groove 31 used to enclose the same embedded part 1 are arranged opposite to each other, and the two side edges of the first groove 21 and the second groove 31 can be connected, so that the first groove 21 and the second groove 31 are combined into a circle. The inner diameter of the circle formed by the first groove 21 and the second groove 31 is slightly larger than or equal to the diameter of the outer circle of the embedded part 1, thereby ensuring the fixing stability of the embedded part 1. The number of the first grooves 21 and the second grooves 31 may be equal or unequal, and the upper substrate 3 and the lower substrate 2 may be staggered, for example, so that the first first groove 21 of the upper substrate 3 and the second second groove 31 of the lower substrate 2 are arranged relative to each other. Of course, according to actual conditions and specific needs, in other embodiments of the present invention, the cross-section of the embedded part 1 is in the shape of a square, and the first groove 21 and the second groove 31 are combined to form a square, which is not the only limitation here.
[0055] Please also refer to Figure 6 As a specific implementation of the method for producing a prefabricated wind turbine blade root provided by the present invention, both the upper substrate 3 and the lower substrate 2 are formed by pultrusion, or only one of the upper substrate 3 or the lower substrate 2 is formed by pultrusion. Specifically, pultrusion is a process method for producing composite material profiles by impregnating continuous fibers or their fabrics with resin under the traction of a traction device and curing the resin by heating a molding die, and the specific processing technology is a conventional process in the prior art. The materials of the upper substrate 3 and the lower substrate 2 are generally multi-axial fibers and thermosetting resins, which can be formed by pultrusion, and can be formed directly without cutting, which can save more materials. Of course, according to actual conditions and specific needs, in other embodiments of the present invention, the upper substrate 3 and / or the lower substrate 2 can also be processed and formed by other methods such as vacuum infusion molding or molding, which is not limited here.
[0056] For further information, see Figure 2 , Figure 3 and Figure 6As a specific embodiment of the method for producing a preformed wind turbine blade root provided by the present invention, the upper substrate 3 has a first fixed cross section 33, and the upper substrate 3 is pultruded by the first fixed cross section 33 along the baseline 34; the lower substrate 2 has a second fixed cross section 23, and the lower substrate 2 is pultruded by the second fixed cross section 23 along the baseline 24. Specifically, the baselines 24 and 34 are arranged perpendicular to the directions of the first fixed cross section 33 and the second fixed cross section 23, and the first fixed cross section 33 and the second fixed cross section 23 can be pultruded along the extending directions of the baselines 24 and 34. The pultrusion direction can be pultruded along the first direction or along the second direction, as long as the shapes of the upper substrate 3 and the lower substrate 2 can be formed.
[0057] Preferably, see Figure 2 , Figure 3 and Figure 6 As a specific embodiment of the method for producing a preformed wind turbine blade root provided by the present invention, the length direction of the first fixed section 33 and the second fixed section 23 is consistent with the length direction of the first groove 21, and the baselines 24 and 34 are perpendicular to the first fixed section 33 and the second fixed section 23. That is, at this time, the length direction of the first fixed section 33 and the second fixed section 23 is the second direction, and then the extension direction of the baseline is the first direction. At this time, the shape of the first fixed section 33 can be consistent with the longitudinal section shape of the upper substrate 3 in the second direction, and the shape of the second fixed section 23 can be consistent with the longitudinal section shape of the lower substrate 2 in the second direction, so it can be stretched and formed at one time. Among them, the shape of the baselines 24 and 34 is formed by splicing several semicircles in sequence, and the connection between the semicircles has a transition arc. The first fixed section 33 and the second fixed section 23 can form a plate body with several grooves along the baselines 24 and 34. The semicircles of the baselines 24 and 34 are the first grooves 21 and the second grooves 31 in the present application. The number of semicircles is the same as the number of the first grooves 21, the second grooves 31 and the embedded parts 1. The embedded parts 1 can be embedded in the first grooves 21 and the second grooves 31.
[0058] Of course, in other embodiments of the present invention, the extension direction of the first fixed section 33 and the second fixed section 23 can also be along the second direction, the baseline 34 or 24 extends along the first direction, and the shape of the first fixed section 33 and the second fixed section 23 can be several semicircles spliced in sequence. At this time, the lower substrate 2 with the first groove 21 and the upper substrate 3 with the second groove 31 can also be stretched. The first substrate and the second substrate can be further processed by cutting or grinding, etc., which is not the only limitation here.
[0059] For further information, see Figure 2 , Figure 3 and Figure 6 As a specific implementation of the method for producing a prefabricated wind turbine blade root provided by the present invention, the shapes of the first fixed section 33 and the second fixed section 23 are both trapezoidal, and one side of the first fixed section 33 and the second fixed section 23 is perpendicular to the bottom side, and the other side is inclined to the bottom side, and the length of the bottom side is greater than the length of the top side. Specifically, the first fixed section 33 and the second fixed section 23 are both right-angled trapezoids, and the side of the first fixed section 33 and the second fixed section 23 close to the embedded part 1 is a right-angle structure, and the side away from the embedded part 1 is inclined. That is, the lower substrate 2 forms an inclined guide surface 22 on the side away from the embedded part 1. The inclined guide surface 22 is a transition slope, which can avoid stress concentration at the end of the lower substrate 2 away from the embedded part 1 when it is connected to other parts of the blade, and avoid damage to the end of the lower substrate 2.
[0060] Further, see Figure 2 , Figure 3 and Figure 6 As a specific embodiment of the method for producing a prefabricated wind turbine blade root provided by the present invention, the length of the first fixed section 33 is less than the length of the second fixed section 23. Specifically, the length of the first fixed section 33 and the second fixed section 23 is equivalent to the length of the upper substrate 3 and the lower substrate 2 in the second direction, that is, the length of the lower substrate 2 in the second direction is greater than the length of the upper substrate 3 in the second direction, the length of the upper substrate 3 in the second direction is greater than the length of the embedded part 1 in the second direction, the length of the lower substrate 2 is longer than the length of the upper substrate 3, and the upper substrate 3 can completely cover the embedded part 1, which can ensure that a stable and complete filling effect can be achieved during the later injection molding filling. The longer length of the lower substrate 2 can facilitate the connection with the blade, increase the area of the connection surface between the root and the blade, and thus achieve a better connection effect. Among them, since the lengths of the embedded part 1 and the upper substrate 3 are both short, the embedded part 1 and the upper substrate 3 are both arranged at one end of the lower substrate 2. Preferably, the thickness of the upper substrate 3 is consistent with the thickness of the lower substrate 2.
[0061] For further information, see Figure 3 As a specific implementation of the method for producing a prefabricated wind turbine blade root provided by the present invention, the method further includes the following steps:
[0062] S3.1 After the embedded part 1 is placed in the first groove 21, a filling piece 5 is arranged on one side of the embedded part 1, and the filling piece 5 is spliced with the embedded part 1 and embedded in the first groove 21 together. Specifically, the material of the filling piece 5 is generally foam or other light and filling material, which is also arranged in the first groove 21, and the filling piece 5 includes a filling rod 51 spliced with the embedded part 1 and a filling lug 52 arranged on opposite sides of the filling rod 51, and the filling lugs 52 of adjacent filling pieces 5 are abutted. The thickness of the filling rod 51 is consistent with the thickness of the embedded part 1, or the thickness of the filling rod 51 is greater than the thickness of the embedded part 1. The filling rod 51 is arranged at one end of the embedded part 1, and the filling lugs 52 are arranged on opposite sides of the filling rod 51, which can prevent the rotation of the filling rod 51 and also play a positioning effect. The filling ears 52 are protruding blocks protruding from both ends of the filling rod 51, and both side ends of the first groove 21 and the second groove 31 can abut against the filling ears 52, and can also play a supporting effect on the position between the first groove 21 and the second groove 31. It can be understood that the filling member 5 can also include a spacer extending between adjacent embedded parts 1, such as a glass fiber reinforced plastic part prefabricated to match the shape of the embedded part, a foam spacer, etc.
[0063] The sum of the length of the filling member 5 and the length of the embedded member 1 is less than the length of the first groove 21. Specifically, the embedded member 1 is arranged at one end of the first groove 21, and the filling member 5 is arranged close to the end of the embedded member 1 and extends to the other end of the first groove 21, thereby playing a filling and supporting effect. The length of the first groove 21 is slightly greater than the total length of the filling member 5 and the embedded member 1, which can ensure a better coating effect.
[0064] Since the end of the lower substrate 2 away from the embedded part 1 has an inclined guide surface 22, the thickness of the filler 5 becomes thinner toward the end away from the embedded part 1, that is, the thickness of the filler 5 becomes thinner toward the end away from the embedded part 1. The filler 5 also forms an inclined surface 32 at this end, thereby playing the role of supporting auxiliary filling support. Among them, the structure of the entire filler 5 is gradually inclined, that is, the thickness of the filler 5 is thinner on the side closer to the inclined guide surface 22, which can not only facilitate the disassembly and assembly between the entire prefabricated part and the blade mold, but also avoid damage caused by stress concentration.
[0065] The end of the upper substrate 3 also has an inclined surface 32, which is used to achieve complete covering of the embedded part 1, and one end of the inclined surface 32 is located on the embedded part 1 and the other end extends to the filling part 5. It can also cover the connection between the embedded part 1 and the filling part 5, thereby ensuring the connection stability between the embedded part 1 and the filling part 5.
[0066] Among them, in order to make the weight of the entire prefabricated part lighter, the upper substrate 3 and the lower substrate 2 generally use materials with strong strength such as limited composite reinforcement materials, but their weight is heavy, and the filler 5 generally uses lightweight materials such as foam, so it is necessary to increase the volume of the filler 5 to reduce the volume of the upper substrate 3 and the lower substrate 2, so the cross-sectional size of the filler 5 can be larger than the cross-sectional size of the embedded part 1, so in order to match the different sizes of the filler 5 and the embedded part 1, and the outer edges of the entire upper substrate 3 and the lower substrate 2 should be smoothly and evenly transitioned, so the corresponding thicknesses of the upper substrate 3 and the lower substrate 2 can be different, that is, it can be divided into a first part that matches the embedded part 1, which has a thicker thickness; and can also include a second part that matches the filler 5, which has a thinner thickness. Of course, according to actual conditions and specific needs, the thickness of the first part and the second part can also be consistent, which is not the only limitation here.
[0067] In order to further reduce the weight of the entire prefabricated part, a filling extension piece (not shown) can be provided between adjacent embedded parts 1, and the filling extension piece can be provided separately or formed by extending the filling piece 5. Since the material weight of the upper substrate 3 and the lower substrate 2 is relatively heavy, and there may be a gap between the upper substrate 3 and the lower substrate 2 located between two adjacent embedded parts 1 due to processing accuracy and other reasons, the gap needs to be filled during the subsequent pouring or bonding, but the weight of the filler is delicate, and the use of a lighter filling extension piece can reduce the weight of the entire prefabricated part, and the material of the filling extension piece is the same as that of the filling piece 5, and foam or other materials with a lighter texture and can be filled can be used.
[0068] Example 2
[0069] The present invention also provides another method for producing a prefabricated blade root of a wind turbine blade, which differs from the method of Example 1 in that: in step S3, the lower substrate 2, the embedded component 1 and the upper substrate 3 are stacked in advance, and then the adhesive is filled between the upper substrate 3 and the lower substrate 2, so that the upper substrate 3, the embedded component 1 and the lower substrate 2 can be bonded. Compared with the method of applying the adhesive multiple times in Example 1, the operation is simpler.
[0070] Example 3
[0071] See also Figure 1 and Figure 7The present invention also provides a mold 6 used in the production method of wind turbine blade root prefabricated parts, the mold 6 includes a lower mold 62 for accommodating the lower substrate 2 and an upper mold 61 for accommodating the upper substrate 3, the lower mold 62 is provided with a plurality of third grooves 621 that fit with the lower surface of the lower substrate 2, the upper mold 61 is provided with a plurality of fourth grooves 611 that fit with the upper surface of the upper mold 61, and an embedded part 1 is coated between the upper substrate 3 and the lower substrate 2. The mold 6 provided by the present invention can place the entire prefabricated part in the mold 6 for production and processing. The height of the entire prefabricated part can be uniformly controlled through the standardized mold 6 to ensure the standardization and uniformity of the processing. By performing pre-hot pressing through the mold 6, the production efficiency can be improved without occupying the blade mold.
[0072] Among them, the lower mold 62 and the upper mold 61 are arranged relative to each other, and the third groove 621 and the fourth groove 611 are also arranged relative to each other, and the lower mold 62 is engaged with the lower surface of the lower substrate 2. Since the lower surface of the lower substrate 2 also has a plurality of protrusions that cooperate with the first groove 21, the lower mold 62 is provided with a plurality of third grooves 621 that cooperate with the protrusions; the upper mold 61 is engaged with the upper surface of the upper substrate 3. Since the upper surface of the upper substrate 3 also has a plurality of protrusions that cooperate with the second groove 31, the upper mold 61 is provided with a plurality of fourth grooves 611 that cooperate with the protrusions. At this time, the third groove 621 and the fourth groove 611 are also arranged in a one-to-one correspondence.
[0073] The upper mold 61 and the lower mold 62 can be opened and closed with each other. Preferably, the upper mold 61 is hinged with the lower mold 62. That is, the upper mold 61 and the lower mold 62 can be two relatively independent molds, or the upper mold 61 and the lower mold 62 can be combined together, that is, the lower mold 62 can remain stationary, and then the upper mold 61 can be movably buckled on the lower mold 62, wherein the connection between the upper mold 61 and the lower mold 62 can also be a rotating connection, or a clamping connection, etc.; or, the upper mold 61 can remain stationary, and the lower mold 62 can be movably buckled on the upper mold 61, which is not limited here.
[0074] The third groove 621 includes a first groove segment 6111 engaged with the upper substrate 3 and a second groove segment 6112 engaged with the filler 5, and an inclined surface 32 is formed at the connection between the first groove segment 6111 and the second groove segment 6112, and the inclined surface 32 is used to fit with the inclined surface 32 at the end of the upper substrate 3.
[0075] Since the length of the upper substrate 3 is shorter than that of the lower substrate 2, the rear half of the lower substrate 2 is in contact with the upper mold 61 through the filler 5, and the filler 5 is also formed with an inclined guide surface 22 at a position opposite to the inclined guide surface 22, which is consistent with the starting position and curvature of the inclined guide surface 22, that is, the inclined convex surface of the third groove 621 can be opposite to the inclined guide surface 22, that is, the starting position and inclination curvature of the inclined guide surface 22 are consistent with the inclined guide surface 22 of the lower substrate 2. At this time, the cooperation between the upper mold 61 and the entire preform can be better achieved.
[0076] Among them, the mold 6 is also provided with other auxiliary infusion components, such as heating elements and control elements. If the adhesive is selected as resin, vacuum infusion may be required. Therefore, the mold 6 also needs to be provided with necessary equipment such as a vacuum port and a vacuum gauge connected to a vacuum machine.
[0077] Example 4
[0078] The present invention also provides a blade root component, which includes an outer fiber fabric 7, an inner fiber fabric 8, and a plurality of mutually spliced prefabricated parts of the wind turbine blade root as described in Example 1 or Example 2, wherein the outer fiber fabric 7 and the inner fiber fabric 8 are respectively coated on opposite sides of the prefabricated parts. There may be a plurality of prefabricated parts, and the plurality of prefabricated parts may be spliced between the outer fiber fabric 7 and the inner fiber fabric 8, and the splicing method may be aligned splicing or staggered splicing.
[0079] Example 5
[0080] See also Figure 8 The present invention also provides a blade root manufacturing method, the blade root manufacturing method comprising the following steps:
[0081] S5. Using the steps in S1 to S4 above to manufacture a plurality of prefabricated wind turbine blade roots as described in any of the above embodiments;
[0082] S6. Laying the outer fiber fabric 7 in the blade root mold, and splicing a plurality of the preforms in sequence; wherein the structure and use method of the blade root mold are the prior art, the outer fiber fabric 7 is laid in the blade root mold, and the outer fiber fabric 7 is generally an external protective layer, and then the preforms are placed on the outer fiber fabric 7;
[0083] Among them, when the prefabricated parts are assembled, all the prefabricated parts can be fixed on a flange (not shown) on the ground in sequence, and then the entire assembled prefabricated parts can be hoisted onto the outer fiber fabric 7; or the assembled prefabricated parts can be directly set on the outer fiber fabric 7, and then the prefabricated parts can be assembled on the spliced outer fiber fabric 7 in sequence and fixed on the flange, which is not the only limitation here.
[0084] S7. Laying an inner layer of fiber fabric 8 on the spliced preforms; the inner layer of fiber fabric 8 is laid on the inner surface of the preforms, which can protect the inner surface of the preforms, and the combination of the inner layer of fiber fabric 8 and the outer layer of fiber fabric 7 can also ensure the effect of injection molding.
[0085] S8. Infusing and molding the blade root in the blade root mold; the infusing and molding method is the existing technology, which can form the inner fiber fabric 8, the outer fiber fabric 7 and the preform into an integrated structure to ensure the connection effect.
[0086] Prefabricate some layers in advance, assemble them and then place them in the blade mold to form an integral part with the remaining layers, which can reduce the difficulty and time of later infusion molding. The block stacking method is adopted in the thickness direction, and multiple sections of prefabricated parts are spliced in the circumferential direction, which can greatly reduce the difficulty of assembly. At the same time, prefabricated parts can be produced in a standardized and modular manner, can be made in advance, and defects can be easily checked and controlled, reducing risks, which can further improve production efficiency, can be universal for different models, and facilitate standardized management.
[0087] The formed blade root can be directly assembled with the blade tip and the blade body at a later stage, or the assembled blade tip and the blade body can be poured and molded again to form a complete blade. The method of pre-forming the blade root can facilitate the later assembly and molding.
[0088] For further information, see Figure 3 and Figure 4 As a specific implementation of the blade manufacturing method provided by the present invention, the splicing method between the prefabricated parts can be aligned splicing or staggered splicing. Specifically, when the prefabricated parts are assembled, they can be aligned splicing, that is, the end of the previous prefabricated part and the head end of the next prefabricated part are directly aligned and spliced, and the assembly method is simple at this time; staggered splicing means that a section of the upper matrix 3 or the lower matrix 2 is reserved at the end of the previous prefabricated part, and there is a partially unsealed area on the next prefabricated part, and the reserved upper matrix 3 or the lower matrix 2 can be connected to the reserved unstitched area, but the operation is more complicated. Of course, according to actual conditions and specific needs, in other embodiments of the present invention, other splicing methods can also be used, which are not limited here.
[0089] Example 6
[0090] The present invention also provides a wind turbine blade, and the wind turbine blade includes a blade tip portion, a blade body portion and a blade root portion, wherein the blade root portion includes the prefabricated part disclosed in Example 3.
[0091] Example 7
[0092] See also Figure 8The present invention also provides a blade manufacturing method, which differs from the blade root manufacturing method in Example 5 in that: the outer fiber fabric 7 is directly laid in the blade mold, and then a plurality of the preforms are spliced in sequence, and then the inner fiber fabric 8 is laid on the spliced preforms; then the relevant parts of the blade tip part and the blade body part are arranged in the blade mold, and poured and formed into a blade in the blade mold.
[0093] At this time, production and processing are carried out directly on the blade mold, which can save the filling process and ensure the tightness of the connection between the blade root part, the blade tip part and the blade body part.
[0094] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for producing a wind turbine blade root assembly, characterized in that: The steps include: Preforming an upper substrate (3) and a lower substrate (2), wherein the upper substrate (3) and the lower substrate (2) are both a single sheet of material, and the lower substrate (2) is provided with a plurality of first grooves (21); The lower layer substrate (2) is placed in a mold (6), a plurality of embedded parts (1) are placed in the first groove (21), and the upper layer substrate (3) is buckled onto the embedded parts (1); Adhesive is coated or laid on the lower substrate (2) and the upper substrate (3) respectively, and bonded to the embedded component (1), or adhesive is filled between the lower substrate (2), the embedded component (1) and the upper substrate (3) to form a composite component; Curing and shaping the assembly in a mold (6); After the embedded component (1) is placed in the first groove (21), a filling component (5) is arranged on one side of the embedded component (1), and at least a portion of the filling component (5) is spliced with the embedded component (1) and embedded in the first groove (21) together; The filling piece (5) comprises a filling rod (51) spliced with the embedded piece (1) and filling ears (52) arranged on opposite sides of the filling rod (51), the filling ears (52) of adjacent filling pieces (5) abut against each other, and the filling ears (52) abut against two side ends of the first groove (21); The lower substrate (2) has an inclined guide surface (22) at one end away from the embedded part (1), the thickness of the filling part (5) becomes thinner towards a section away from the embedded part (1), and the filling part (5) has an inclined surface (32) towards a section away from the embedded part (1).
2. The method for producing a wind turbine blade root assembly according to claim 1, characterized in that: The upper matrix (3) and / or the lower matrix (2) are fiber-reinforced composite materials.
3. The method for producing a wind turbine blade root assembly according to claim 2, characterized in that: The upper substrate (3) and / or the lower substrate (2) are formed by pultrusion.
4. The method for producing a wind turbine blade root assembly according to claim 3, characterized in that: The lower layer substrate (2) has a second fixed cross section (23), and the lower layer substrate (2) is pultruded along the base line (24) from the second fixed cross section (23); The upper substrate (3) has a first fixed cross section (33), and the upper substrate (3) is pultruded along a base line (34) from the first fixed cross section (33).
5. The method for producing a wind turbine blade root assembly according to claim 4, characterized in that: The length direction of the first fixed section (33) and the second fixed section (23) is consistent with the length direction of the first groove (21), and the base lines (24 and 34) are perpendicular to the first fixed section (33) and the second fixed section (23).
6. The method for producing a wind turbine blade root assembly according to claim 5, characterized in that: The shape of the first fixed cross section (33) and / or the second fixed cross section (23) is a trapezoid.
7. The method for producing a wind turbine blade root assembly according to claim 5, characterized in that: The length of the first fixing cross section (33) is smaller than the length of the second fixing cross section (23).
8. The method for producing a wind turbine blade root assembly according to claim 5, characterized in that: The second fixed cross section (23) comprises a first portion corresponding to the embedded part (1) and a second portion corresponding to the filling part (5) in the first groove (21), and the first portion and the second portion have different thicknesses.
9. The method for producing a wind turbine blade root assembly according to claim 5, characterized in that: The sum of the length of the filling piece (5) in the first groove (21) and the length of the embedded part (1) is smaller than the length of the first groove (21).
10. The method for producing a wind turbine blade root assembly according to any one of claims 1 to 9, characterized in that: Filling extension pieces are provided between adjacent embedded pieces (1).
11. The method for producing a wind turbine blade root assembly according to any one of claims 1 to 9, characterized in that: A plurality of second grooves (31) are provided on the upper substrate (3), and the first grooves (21) and the second grooves (31) are arranged opposite to each other and are surrounded on the outside of the embedded part (1).
12. A mold, used in the method for producing a wind turbine blade root assembly according to any one of claims 1 to 11, characterized in that: It comprises a lower mould (62) for accommodating the lower substrate (2) and an upper mould (61) for accommodating the upper substrate (3); the lower mould (62) is provided with a plurality of third grooves (621) which fit with the lower surface of the lower substrate (2).
13. The mold according to claim 12, characterized in that: The upper mold (61) is rotatably connected to the lower mold (62), and a plurality of fourth grooves (611) are provided in the upper mold (61) and are fitted with the upper surface of the upper substrate (3).