Buried structure high linearity DFB laser chip for optical communication and preparation method thereof
By growing an epitaxial structure and forming a ridge structure on a semi-insulating substrate, combined with high-temperature baking and coplanar electrode design, the problems of poor carrier confinement capability and Al material oxidation of high-linearity DFB lasers at high temperatures are solved, achieving a better High reliability and efficiency.
Patent Information
- Application Number
- CN202010167005.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-03-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-11
AI Technical Summary
Existing high-linearity DFB lasers have poor carrier confinement capabilities at high temperatures, and the Al material has oxidation and reliability problems when exposed to air, resulting in low operating efficiency of the device at high temperatures and high currents.
By growing an epitaxial structure on a semi-insulating substrate, a uniform grating is prepared using a holographic method and re-grown to form a ridge structure. A single layer of SiN is used as a mask layer and a ridge waveguide is formed through chemical etching, and the surface is removed by high-temperature baking. particles and oxide layers, and finally prepare coplanar electrodes to improve carrier injection efficiency and device reliability.
It effectively improves the reliability and high-temperature performance of the laser, increases the carrier injection efficiency, reduces non-radiative coincidence and heat generation, and improves the overall performance and cost-effectiveness of the device.
Smart Images

Figure CN111181005B_ABST
Abstract
Description
[0001] Technology Neighborhood:
[0002] The present invention relates to a buried structure high linearity DFB laser chip for optical communication and a preparation method thereof, and in particular to the preparation of a buried structure laser containing Al material by optimizing and adjusting aspects such as epitaxial structure, surface treatment of material growth, and chip structure, and effectively improving laser reliability optimization, optimizing the carrier injection process, and improving heat generation and high temperature performance. Background technology:
[0004] High linearity DFB lasers are widely used in cable TV, backbone networks, space optical communications and other fields. The linearity of the laser is usually improved by increasing the output power of the laser. Generally, the InP / InGaAsP material system and buried structure are used to prepare high linearity lasers. However, due to the characteristics of the InGaAsP material structure, its high temperature carrier confinement ability is relatively poor; AlGaInAs material has a larger conduction band quantum well energy level difference and a lower valence band quantum well energy level difference, which makes the electron confinement effect at high temperature better, and the distribution of heavy holes in the quantum well is more uniform, which is more conducive to improving the high temperature performance of the device; however, in conventional applications, due to the oxidation and reliability problems of Al material exposed to air, the InP / AlGaInAs material system generally uses a ridge structure to prepare the waveguide in practical applications, which also makes this chip have the problem of poor lateral carrier confinement ability. Summary of the invention:
[0006] The object of the present invention is to provide a buried structure high linearity DFB laser chip for optical communication and a preparation method thereof. The buried structure high linearity DFB laser chip for optical communication and a preparation method thereof realize the preparation of a buried structure laser containing Al material by optimizing and adjusting the epitaxial structure, surface treatment of material growth, chip structure and other aspects, and effectively improve the laser reliability optimization, optimize the carrier injection process, and improve the heat generation and high temperature performance.
[0007] The method for preparing a buried structure high linearity DFB laser chip for optical communication of the present invention is characterized by: (1) growing the primary epitaxial structure of the laser on a semi-insulating substrate, preparing a uniform grating by a holographic method, and regrowing the grating; (2) using a single layer of SiN as a mask to form a ridge structure, and using a chemical etching method to form a ridge waveguide, then treating the surface of the ridge waveguide, and sequentially completing the growth of a current blocking layer and removing SiN in an epitaxial device; then completing the final growth; (3) preparing P-type and N-type electrodes on the sample surface to form a coplanar electrode structure, and then performing subsequent process preparation on the laser to complete the chip preparation process.
[0008] Further, in step (1): a two-inch semi-insulating InP substrate is placed in an MOCVD chamber, baked at high temperature, and PH3 is introduced to remove particles on the substrate surface and improve the surface growth quality; then P-InP, N-InP and P-InP structures are grown to further suppress the diffusion of current to the substrate; then the following are grown in sequence: N-InP buffer layer, N-InAlAs electron blocking layer, undoped AlGaInAs lower waveguide layer, AlGaInAs strained multi-quantum well and barrier structure, undoped AlGaInAs upper waveguide layer, P-InAlAs electron blocking layer, P-InP spacer layer, P-InGaAsP grating layer, P-InP protective layer, to complete a re-growth; then a uniform grating is prepared on the wafer surface by holographic exposure and chemical etching, and the grating etching depth penetrates the P-InGaAsP grating layer; then the grating cover layer structure: P-InP, P-InGaAs, P-InP is grown to complete the buried re-growth of the grating.
[0009] Further, in step (2): 400 nm of SiN, a SiN ridge structure is formed by photolithography, etching and corrosion, and then the wafer is isotropically etched with a bromine-based etching solution at low temperature to a depth of N-InP buffer layer; then the wafer is etched in 10% HF for about 3 minutes, then the wafer is rinsed with deionized water, blown dry with nitrogen, and quickly placed in the prepared MOCVD chamber; before growth, the wafer is baked at three temperature points: 450°C, 550°C, and 650°C, and a large amount of AsH3 / H2 gas is introduced at the same time. The high-temperature baking process under the temperature gradient combination effectively removes particles, dirt and oxide layer structures on the surface of the Al-containing material and improves the surface quality of the material growth, which is a key point for improving the reliability of the Al-containing buried structure laser; then P-InP / N-InP / P-InP current blocking layers are grown in sequence to form a lateral confinement effect on carriers; finally, the dielectric layer on the surface of the wafer is removed, and a P-InP space layer, an InGaAsP transition layer and a P-InGaAs ohmic contact layer are grown in sequence to complete the epitaxial growth of the material.
[0010] Furthermore, in step (3): P-type and N-type electrodes are prepared on the upper surface of the sample to form coplanar electrodes, thereby effectively reducing the carrier injection path, improving the injection efficiency, reducing heat generation, and improving high-temperature characteristics; the specific process is: a bromine-based etching solution is used to etch the N-type InP buffer layer on both sides of the buried ridge to form a table structure, one side of the table is a groove, and a ridge opening is prepared on one side of the groove to form a P-side electrode, and an N-side electrode is prepared on the other side of the table. The N / P type electrodes use the same Ti / Pt / Au metal to further reduce costs; finally, the prepared chip is dissociated into bars, and a high-reflection and high-transmittance optical film is evaporated on the cavity surface to complete the chip preparation.
[0011] The present invention provides a method for preparing a buried structure high linearity DFB laser chip for optical communication, characterized in that: firstly, a PNP is grown on a semi-insulating InP substrate. InP electron blocking layer, N-InP buffer layer, waveguide structure, strained AlGaInAs multiple quantum well and grating layer; then prepare the grating and bury the grating and re-grow it, use a single layer of SiN as a mask layer to prepare a ridge structure, then use a bromine-based etching solution to etch the ridge structure until the substrate layer is etched to form a ridge waveguide structure, and the SiN on the ridge waveguide forms a cantilever; place the sample in an HF solution for etching, and use the slow etching rate of SiN to remove the oxides on both sides of the ridge waveguide; then quickly place the sample in the prepared MOCVD cavity for electron blocking structure re-growth, and before growth, use 450℃, 550℃, and 650℃ to bake the wafer to remove the particle dirt and oxide layer on the surface of the wafer, especially the surface of the aluminum-containing material structure, and introduce a large amount of AsH3 / H2 during baking to suppress the volatilization of As in the AlGaInAs material; baking removes dirt and oxide layer, while improving the growth quality of the sample surface, and then grows PNP InP electron blocking layer structure; HF solution is used to etch and remove SiN on the sample surface, and a P-InP space layer, a P-InGaAsP transition structure and a P-InGaAs ohmic contact layer are finally grown in an MOCVD device to complete epitaxial growth; then the electrode structure of the laser is prepared, a groove structure is prepared on one side of the ridge structure, and a hole is opened on the ridge to form a P-side electrode; and on the other side of the ridge, the N-InP buffer layer is etched to prepare an N-type electrode, thereby forming an N-side electrode, forming a structure in which the N-side and P-side electrodes are coplanar.
[0012] The buried structure high linearity DFB laser chip for optical communication of the present invention is characterized in that: the preliminary structure of the laser chip manufacturing process includes, from bottom to top, a semi-insulating InP substrate layer, a P-InP, an N-InP, a P-InP current blocking structure layer and an N-InP buffer layer; above the N-InP buffer layer, from bottom to top, in the growth order, the following are: an N-InAlAs electron blocking layer, an AlGaInAs lower waveguide layer, an AlGaInAs strained multi-quantum well and barrier structure layer, an AlGaInAs upper waveguide layer, a P-InAlAs electron blocking layer, a P-InP spacer layer, a P-InGaAsP grating layer, a P-InP layer, a P-InGaAs layer and a P-InP layer; a SiN dielectric layer is provided on the P-InP layer, and a ridge waveguide structure is formed from the upper part of the N-InP buffer layer to the P-InP layer; and the SiN dielectric layer forms a cantilever structure on the ridge waveguide.
[0013] Furthermore, the structure before the formation of the above-mentioned laser chip manufacturing process includes, on the preliminary structure, sequentially growing a P-InP current blocking layer, an N-InP current blocking layer, and a P-InP current blocking layer from bottom to top beside the ridge waveguide structure, removing the SiN dielectric layer, and then sequentially growing a P-InP space layer, an InGaAsP transition layer, and a P-InGaAs ohmic contact layer on the P-InP current blocking layer, forming a table structure on the P-InGaAs ohmic contact layer, providing an opening on the table, forming a P-type electrode on the table and on the left side of the table; and forming an N-type electrode by opening a hole in the area on the right side of the table.
[0014] The present invention adopts an effective surface treatment process, and further adopts a step-by-step high-temperature baking process to further remove particles, dirt and oxide layers formed during the Al material process and exposed to the air, effectively improving the reliability problem of the buried structure laser containing Al material; in addition, the working efficiency of the laser under high temperature or high current has always been a difficult problem. In addition to adopting the characteristics of the Al-containing material itself and the characteristics of the buried structure, the present invention adds a PNP current limiting layer on the semi-insulating substrate to further improve the longitudinal limiting ability of the carriers. In addition, the method of further adopting the coplanar electrode can further improve the injection efficiency of the carriers for the laser working under high current, thereby reducing non-radiative coincidence and heat generation, and improving the reliability problem caused by heat problems; in addition, the use of the coplanar electrode can complete the preparation of the P-side and N-side electrodes in a single step and does not require a physical thinning process, further reducing the overall preparation cost of the chip. Description of the drawings:
[0016] Figure 1 This is a diagram of the laser structure after chemical etching to form a ridge waveguide, in which 1 is a semi-insulating InP substrate, 2 is a P / N / P-InP current blocking structure, 3 is an N-InP buffer layer, and 4 are, from bottom to top in the growth order: N-InAlAs electron blocking layer 41, AlGaInAs lower waveguide layer 42, AlGaInAs strained multiple quantum well and barrier structure 43, AlGaInAs upper waveguide layer 44, P-InAlAs electron blocking layer 45, P-InP spacer layer 46, P-InGaAsP grating layer 47, P-InP layer 48, P-InGaAs layer 49 and P-InP layer 410; 5 is a SiN dielectric layer, which forms a cantilever structure on the ridge waveguide.
[0017] Figure 2 This is the structure diagram of the laser before preparing the metal electrode. Figure 2 6 in Figure 1Removing the SiN structure, 7 is a P-InP current blocking layer, 8 is an N-InP current blocking layer, and 9 along the growth direction from bottom to top are: P-InP current blocking layer 91, P-InP space layer 92, P-InGaAsP transition layer 93, P-InGaAs ohmic contact layer 94; 10 is a formed mesa structure with a mesa width of about 10 microns. A hole is opened on the mesa, and a P-type electrode is formed on the mesa and on the left side of the mesa; a hole is opened in the area about 11 on the right side of the mesa to form an N-type electrode. Specific implementation method:
[0019] The present invention discloses a method for preparing a buried structure high linearity DFB laser chip for optical communication, comprising: (1) growing a primary epitaxial structure of the laser on a semi-insulating substrate, preparing a uniform grating by a holographic method, and regrowing the grating; (2) using a single layer of SiN as a mask to form a ridge structure, and forming a ridge waveguide by a chemical etching method, and then treating the surface of the ridge waveguide, and sequentially completing the growth of a current blocking layer and removing SiN in an epitaxial device; and then completing the final growth; and (3) preparing P-type and N-type electrodes on the sample surface to form a coplanar electrode structure, and then performing subsequent process preparation on the laser to complete the chip preparation process.
[0020] In step (1): a two-inch semi-insulating InP substrate is placed in a MOCVD chamber, baked at high temperature, and PH3 is introduced to remove particles on the substrate surface and improve the surface growth quality; then P-InP, N-InP and P-InP structures are grown to further suppress the diffusion of current to the substrate; then the following are grown in sequence: N-InP buffer layer, N-InAlAs electron blocking layer, undoped AlGaInAs lower waveguide layer, AlGaInAs strained multi-quantum well and barrier structure, undoped AlGaInAs upper waveguide layer, P-InAlAs electron blocking layer, P-InP spacer layer, P-InGaAsP grating layer, P-InP protective layer, to complete a re-growth; then a uniform grating is prepared on the wafer surface by holographic exposure and chemical etching, and the grating etching depth penetrates the P-InGaAsP grating layer; then the grating cover layer structure: P-InP, P-InGaAs, P-InP is grown to complete the buried re-growth of the grating.
[0021] In step (2): 400nm is deposited by PECVD SiN, a SiN ridge structure is formed by photolithography, etching and corrosion, and then the wafer is isotropically etched with a bromine-based etching solution at low temperature to a depth of N-InP buffer layer; then the wafer is etched in 10% HF for about 3 minutes, then the wafer is rinsed with deionized water, blown dry with nitrogen, and quickly placed in the prepared MOCVD chamber; before growth, the wafer is baked at three temperature points: 450°C, 550°C, and 650°C, and a large amount of AsH3 / H2 gas is introduced at the same time. The high-temperature baking process under the temperature gradient combination effectively removes particles, dirt and oxide layer structures on the surface of the Al-containing material and improves the surface quality of the material growth, which is a key point for improving the reliability of the Al-containing buried structure laser; then P-InP / N-InP / P-InP current blocking layers are grown in sequence to form a lateral confinement effect on carriers; finally, the dielectric layer on the surface of the wafer is removed, and a P-InP space layer, an InGaAsP transition layer and a P-InGaAs ohmic contact layer are grown in sequence to complete the epitaxial growth of the material.
[0022] In step (3): P-type and N-type electrodes are prepared on the upper surface of the sample to form coplanar electrodes, thereby effectively reducing the carrier injection path, improving the injection efficiency, reducing heat generation, and improving high-temperature characteristics; the specific process is: a bromine-based etching solution is used to etch the N-type InP buffer layer on both sides of the buried ridge to form a table structure, one side of the table is a groove, and a ridge opening is prepared on one side of the groove to form a P-side electrode, and an N-side electrode is prepared on the other side of the table. The N / P type electrodes use the same Ti / Pt / Au metal to further reduce costs; finally, the prepared chip is dissociated into bars, and a high-reflection and high-transmittance optical film is evaporated on the cavity surface to complete the chip preparation.
[0023] The method for preparing a buried structure high linearity DFB laser chip for optical communication of the present invention is as follows: firstly, a PNP is grown on a semi-insulating InP substrate. InP electron blocking layer, N-InP buffer layer, waveguide structure, strained AlGaInAs multiple quantum well and grating layer; then prepare the grating and bury the grating and re-grow it, use a single layer of SiN as a mask layer to prepare a ridge structure, then use a bromine-based etching solution to etch the ridge structure until the substrate layer is etched to form a ridge waveguide structure, and the SiN on the ridge waveguide forms a cantilever; place the sample in an HF solution for etching, and use the slow etching rate of SiN to remove the oxides on both sides of the ridge waveguide; then quickly place the sample in the prepared MOCVD cavity for electron blocking structure re-growth, and before growth, use 450℃, 550℃, and 650℃ to bake the wafer to remove the particle dirt and oxide layer on the surface of the wafer, especially the surface of the aluminum-containing material structure, and introduce a large amount of AsH3 / H2 during baking to suppress the volatilization of As in the AlGaInAs material; baking removes dirt and oxide layer, while improving the growth quality of the sample surface, and then grows PNP InP electron blocking layer structure; HF solution is used to etch and remove SiN on the sample surface, and a P-InP space layer, a P-InGaAsP transition structure and a P-InGaAs ohmic contact layer are finally grown in an MOCVD device to complete epitaxial growth; then the electrode structure of the laser is prepared, a groove structure is prepared on one side of the ridge structure, and a hole is opened on the ridge to form a P-side electrode; and on the other side of the ridge, the N-InP buffer layer is etched to prepare an N-type electrode, thereby forming an N-side electrode, forming a structure in which the N-side and P-side electrodes are coplanar.
[0024] Here are the steps in more detail:
[0025] The two-inch Fe-doped InP substrate 1 was placed in a MOCVD chamber and baked at 590°C for 15 min, with PH3 gas continuously introduced during the baking process; then the growth thickness was 50 nm and the doping concentration was 10 18 , 2×10 18 , 10 18The P-InP, N-InP, and P-InP structures 2 are further used to suppress the diffusion of current to the substrate; then the following are grown in sequence: a 1500nm N-InP buffer layer 3, a 50nm N-InAlAs electron blocking layer 41, an 80nm undoped AlGaInAs lower waveguide layer 42, an AlGaInAs strained multiple quantum well and barrier structure 43, wherein the thickness of the well and the barrier are 5nm and 8nm respectively, the number of quantum well layers is 4, an 80nm undoped AlGaInAs upper waveguide layer 44, a 50nm P-InAlAs electron blocking layer 45, a 50nm P-InP spacer layer 46, a 5nm P-InGaAsP grating layer 47, and a 15nm P-InP protective layer, to complete a re-growth; then a uniform grating is prepared on the surface of the wafer by holographic exposure and chemical etching, and the grating etching depth penetrates the P-InGaAsP grating layer 47; then the grating cover layer structure is grown: a 50nm P-InP layer 48, a 50nm The P-InGaAs layer 49 and the 50nm P-InP layer 410 complete the buried regrowth of the grating.
[0026] A 400 nm SiN dielectric layer 5 is deposited by PECVD, and a SiN ridge structure is formed by photolithography, etching and chemical etching. The width of the SiN strip is about 3.5 μm. Then, a bromine-based etching solution is used to isotropically etch the wafer at a low temperature to a depth of the N-InP buffer layer 3 to form a ridge waveguide structure (such as Figure 1 As shown in the figure, the width of the quantum well region is about 2 microns; the wafer is placed in 10% HF for about 3 minutes to remove the surface oxide, rinsed with deionized water, dried with nitrogen, and immediately placed in the prepared MOCVD chamber; before growth, it is baked at 450°C, 550°C, and 650°C for 20 minutes respectively, and a large amount of AsH3 / H2 (100 / 5000sccm) gas is introduced during the baking process, and the baking temperature is gradually increased to achieve the purpose of removing particles, dirt and oxide layers on the surface of the sample; then, a P-InP current blocking layer 7, an N-InP current blocking layer 8, and a P-InP current blocking layer 91 (500 / 1000 / 200nm) are grown in sequence, and the current blocking layer forms a lateral confinement effect on the carriers; finally, the dielectric layer on the surface of the wafer is removed, and a 50nm P-InP space layer 92, a 50nm InGaAsP transition layer 93, and a 50nm P-InGaAs ohmic contact layer 94 are grown in sequence to complete the epitaxial growth of the material.
[0027] A 150nm SiO2 dielectric layer 5 is deposited by PECVD, and a SiO2 opening area on the surface is formed by photolithography, etching and chemical etching. A bromine-based etching solution is used to stir and etch the N-type InP buffer layer 3 at low temperature to form a SiO2 opening area on the surface. Figure 2The chip structure shown in the figure is to remove the SiO2 layer on the surface of the chip and deposit a 400nm SiO2 passivation layer by PECVD. Figure 2 The countertops and Figure 2 A hole is opened in the middle area 11, and a metal electrode is evaporated to form an ohmic contact with an alloy; the chip is dissociated into bars with a cavity length of 1000 microns, and a high-transmittance and high-reflection optical film is evaporated on the light-emitting end face and the backlight end face of the laser to complete the chip preparation.
Claims
1. A method for preparing a buried structure high linearity DFB laser chip for optical communication, characterized in that: (1) growing the laser primary epitaxial structure on a semi-insulating substrate, preparing a uniform grating by a holographic method, and regrowing the grating; (2) using a single layer of SiN as a mask to form a ridge structure, and using a chemical etching method to form a ridge waveguide, then treating the surface of the ridge waveguide, and sequentially completing the growth of a current blocking layer and removing SiN in the epitaxial device; then completing the final growth; (3) preparing P-type and N-type electrodes on the sample surface to form a coplanar electrode structure, and then performing subsequent process preparation on the laser to complete the chip preparation process; in step (3): preparing on the upper surface of the sample P-type and N-type electrodes form coplanar electrodes, which effectively reduces the carrier injection path, improves injection efficiency, reduces heat, and improves high-temperature characteristics; the specific process is: a bromine-based etching solution is used to etch the N-type InP buffer layer on both sides of the buried ridge to form a table structure, one side of the table is a groove, and a ridge opening is prepared on one side of the groove to form a P-side electrode, and an N-side electrode is prepared on the other side of the table. The N / P type electrodes use the same Ti / Pt / Au metal to further reduce costs; finally, the prepared chip is dissociated into bars, and a high-reflection and high-transmittance optical film is evaporated on the cavity surface to complete the chip preparation.
2. The method for preparing a buried structure high linearity DFB laser chip for optical communication according to claim 1, characterized in that: In step (1): a two-inch semi-insulating InP substrate is placed in a MOCVD chamber, baked at high temperature, and PH3 is introduced to remove particles on the substrate surface and improve the surface growth quality; then P-InP, N-InP and P-InP structures are grown to further suppress the diffusion of current to the substrate; then the following are grown in sequence: N-InP buffer layer, N-InAlAs electron blocking layer, undoped AlGaInAs lower waveguide layer, AlGaInAs strained multi-quantum well and barrier structure, undoped AlGaInAs upper waveguide layer, P-InAlAs electron blocking layer, P-InP spacer layer, P-InGaAsP grating layer, P-InP protective layer, to complete a re-growth; then a uniform grating is prepared on the wafer surface by holographic exposure and chemical etching, and the grating etching depth penetrates the P-InGaAsP grating layer; then the grating cover layer structure: P-InP, P-InGaAs, P-InP is grown to complete the buried re-growth of the grating.
3. The method for preparing a buried structure high linearity DFB laser chip for optical communication according to claim 1, characterized in that: In step (2): 400nm is deposited by PECVD SiN, a SiN ridge structure is formed by photolithography, etching and corrosion, and then the wafer is isotropically etched with a bromine-based etching solution at low temperature to a depth of N-InP buffer layer; then the wafer is etched in 10% HF for 3 minutes, then the wafer is rinsed with deionized water, blown dry with nitrogen, and quickly placed in the prepared MOCVD chamber; before growth, the wafer is baked at three temperature points: 450°C, 550°C, and 650°C, and a large amount of AsH3 / H2 gas is introduced at the same time. The high-temperature baking process under the temperature gradient combination effectively removes particles, dirt and oxide layer structures on the surface of the Al-containing material and improves the surface quality of the material growth, which is a key point for improving the reliability of the Al-containing buried structure laser; then P-InP / N-InP / P-InP current blocking layers are grown in sequence to form a lateral confinement effect on carriers; finally, the dielectric layer on the wafer surface is removed, and a P-InP space layer, an InGaAsP transition layer and a P-InGaAs ohmic contact layer are grown in sequence to complete the epitaxial growth of the material.
4. A method for preparing a buried structure high linearity DFB laser chip for optical communication, characterized in that: First, a PNP InP electron blocking layer, an N-InP buffer layer, a waveguide structure, a strained AlGaInAs multiple quantum well and a grating layer are grown on a semi-insulating InP substrate; then a grating is prepared and buried and regrown, a single layer of SiN is used as a mask layer to prepare a ridge structure, and then a bromine-based etching solution is used to etch the ridge structure until the substrate layer is etched to form a ridge waveguide structure, and the SiN on the ridge waveguide forms a cantilever; the sample is placed in an HF solution for etching, and the slow etching rate of SiN is used to remove the oxide on both sides of the ridge waveguide; then the sample is quickly placed in a prepared MOCVD cavity for electron blocking structure re-growth, and before growth, the wafer is baked at 450°C, 550°C and 650°C to remove particle dirt and oxide layer on the surface of the aluminum-containing material structure, and a large amount of AsH3 / H2 is introduced during baking to suppress the volatilization of As in the AlGaInAs material; baking removes dirt and oxide layer, while improving the growth quality of the sample surface, and then the PNP is grown InP electron blocking layer structure; HF solution is used to etch and remove SiN on the sample surface, and a P-InP space layer, a P-InGaAsP transition structure and a P-InGaAs ohmic contact layer are finally grown in an MOCVD device to complete epitaxial growth; then the electrode structure of the laser is prepared, a groove structure is prepared on one side of the ridge structure, and a hole is opened on the ridge to form a P-side electrode; and on the other side of the ridge, the N-InP buffer layer is etched to prepare an N-type electrode, thereby forming an N-side electrode, forming a structure in which the N-side and P-side electrodes are coplanar.
5. A buried structure high linearity DFB laser chip for optical communication obtained by any preparation method of claims 1-4, characterized in that: The preliminary structure of the laser chip manufacturing process includes, from bottom to top, a semi-insulating InP substrate layer (1), a P-InP, an N-InP, a P-InP current blocking structure layer (2), and an N-InP buffer layer (3). Above the N-InP buffer layer (3), the following growth order from bottom to top are: an N-InAlAs electron blocking layer (41), an AlGaInAs lower waveguide layer (42), an AlGaInAs strained multi-quantum well and barrier structure layer (43), and an AlGaInAs upper waveguide layer (44). , a P-InAlAs electron blocking layer (45), a P-InP spacer layer (46), a P-InGaAsP grating layer (47), a first P-InP layer (48), a P-InGaAs layer (49) and a second P-InP layer (410); a SiN dielectric layer (5) is provided on the second P-InP layer (410); a ridge waveguide structure is formed from the upper part of the N-InP buffer layer (3) to the second P-InP layer (410); and the SiN dielectric layer (5) forms a cantilever structure on the ridge waveguide.
6. The buried structure high linearity DFB laser chip for optical communication according to claim 5, characterized in that: The structure before forming in the laser chip manufacturing process includes: on a preliminary structure (6), a first P-InP current blocking layer (7), an N-InP current blocking layer (8), and a second P-InP current blocking layer (91) are sequentially grown from bottom to top beside a ridge waveguide structure; after removing a SiN dielectric layer (5), a P-InP space layer (92), an InGaAsP transition layer (93), and a P-InGaAs ohmic contact layer are sequentially grown on the second P-InP current blocking layer (91); a table structure (10) is formed on the P-InGaAs ohmic contact layer; an opening is provided on the table; a P-type electrode is formed on the table and on the left side of the table; and an opening is formed in a region (11) on the right side of the table to form an N-type electrode.