Wear-resistant and scratch-resistant film and preparation method thereof
By forming a thin film structure of substrate, metal base layer, transition layer and color layer on the surface of electronic equipment, combined with magnetron sputtering technology, the problem of insufficient film density and hardness in the existing technology is solved, and high wear resistance and protection is achieved Scraping performance and various colors.
Patent Information
- Application Number
- CN202010499575.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-06-04
AI Technical Summary
The density and hardness of the surface decorative film of existing electronic equipment is insufficient, making it difficult to meet the needs of high wear resistance, scratch resistance and diverse colors.
Using a thin film structure including a substrate, a metal base layer, a first transition layer, a second transition layer and a color layer, a titanium chromium transition layer is formed through magnetron sputtering technology, combining medium frequency and high-power pulse magnetron sputtering power supply to improve The density and hardness of the film.
It achieves good bonding force and high wear resistance and scratch resistance between the film layers, and at the same time displays a variety of colors, solving the problem of insufficient film density and hardness.
Smart Images

Figure CN111519155B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thin films, and in particular to a wear-resistant and scratch-resistant thin film and a preparation method thereof. Background Art
[0002] With the development of society and the advancement of manufacturing technology, electronic devices are becoming more and more popular, especially portable electronic devices, which are appearing in all aspects of people's lives, such as smart phones, watches, tablet computers, cameras, etc. While developing and using these devices, researchers and consumers have higher and higher performance requirements for these devices. In addition to hoping that these devices have multiple functions and good reliability, they also hope that these devices have good wear and scratch resistance, and can also present a variety of colors. When these devices are hit and rubbed during use, they can still maintain stable performance.
[0003] However, conventional electronic equipment surface decoration films are not dense enough and hard enough to meet the above requirements. Summary of the invention
[0004] Based on this, it is necessary to provide a wear-resistant and scratch-resistant film, which has good wear-resistant and scratch-resistant properties and can present various colors.
[0005] In addition, it is also necessary to provide a method for preparing a wear-resistant and scratch-resistant film, which can effectively improve the bonding force between the layers of the wear-resistant and scratch-resistant film and effectively improve the wear-resistant and scratch-resistant performance of the film.
[0006] In order to solve the above problems, the specific technical solution of the present invention is:
[0007] One object of the present invention is to provide a wear-resistant and scratch-resistant film, the wear-resistant and scratch-resistant film comprising a substrate, a metal primer layer, a first transition layer, a second transition layer and a color layer;
[0008] The metal primer layer has a bonding surface for bonding to the surface of the substrate and a functional surface arranged opposite to the bonding surface; the first transition layer is located on the functional surface, and the second transition layer is located on the surface of the first transition layer away from the metal primer layer; the color layer is located on the surface of the second transition layer away from the first transition layer;
[0009] The second transition layer is a titanium-chromium transition layer.
[0010] In one embodiment, the thickness ratio of the metal base layer, the first transition layer, the second transition layer and the color layer is (1-3):(6-10):1:(3-5).
[0011] In one embodiment, the thickness of the second transition layer is 0.05 μm to 0.2 μm.
[0012] In one embodiment, the metal base layer is a metal Ti base layer, a metal Cr base layer or a metal TiCr base layer.
[0013] In one embodiment, the first transition layer is a TiCrN transition layer, a CrN transition layer or a TiN transition layer.
[0014] In one embodiment, the second transition layer is a TiCrCN transition layer or a TiCrN transition layer.
[0015] In one of the embodiments, the color layer is a TiCrCN color layer, a TiCrN color layer or a TiN color layer.
[0016] Another object of the present invention is to provide a method for preparing a wear-resistant and scratch-resistant film, the preparation method comprising the following steps:
[0017] A metal primer layer is formed on a substrate; a first transition layer is formed on a surface of the metal primer layer by a first magnetron sputtering; a second transition layer is formed on a surface of the first transition layer by a second magnetron sputtering; and a color layer is formed on a surface of the second transition layer by a third magnetron sputtering;
[0018] The second transition layer is a titanium-chromium transition layer;
[0019] In the second magnetron sputtering, the titanium target is connected to a high-power pulse magnetron sputtering power supply, the power of which is 5kW to 10kW and the current is 100A to 500A; the chromium target is connected to a medium-frequency magnetron sputtering power supply, the power of which is 3kW to 12kW.
[0020] In one of the embodiments, the first magnetron sputtering adopts a medium frequency magnetron sputtering power supply, and the power of the medium frequency magnetron sputtering power supply is 3kW to 12kW; the third magnetron sputtering adopts a high power pulsed magnetron sputtering power supply, and the power of the high power magnetron sputtering power supply is 5kW to 10kW and the current is 100A to 500A.
[0021] In one of the embodiments, a medium frequency magnetron sputtering power source is used to form the metal base layer on the substrate, and the power of the medium frequency magnetron sputtering power source is 3 kW to 12 kW.
[0022] The wear-resistant and scratch-resistant film comprises a substrate, a metal base layer, a first transition layer, a second transition layer and a color layer. The metal base layer has a bonding surface for bonding to the surface of the substrate and a functional surface arranged opposite to the bonding surface; the first transition layer is located on the functional surface, the second transition layer is located on the surface of the first transition layer away from the metal base layer; the color layer is located on the surface of the second transition layer away from the first transition layer. The second transition layer is a titanium-chromium transition layer. The above-mentioned film has good bonding force between the film layers through the structural design of the substrate, the metal base layer, the first transition layer, the second transition layer and the color layer, and the film has good wear-resistant and scratch-resistant performance. At the same time, the above-mentioned wear-resistant and scratch-resistant film can display a variety of colors. Specifically, the metal base layer is used as the base layer, which provides a stable support for the overall structure of the film. At the same time, the metal base layer can effectively improve the bonding strength between the substrate and the transition layer, so that the film can show stable performance. The arrangement of the first transition layer, the second transition layer and the color layer makes the film show the characteristics of being dense and hard, so that the film shows good wear-resistant and scratch-resistant performance. Furthermore, a titanium-chromium transition layer is provided between the first transition layer and the color layer, which can ensure stress matching and element matching between the first transition layer and the color layer, further enhance the bonding force between the first transition layer, the second transition layer and the color layer, and further improve the wear resistance and scratch resistance of the film.
[0023] The preparation method of the wear-resistant and scratch-resistant film comprises the following steps: forming a metal base layer on the surface of the substrate; forming a first transition layer on the surface of the metal base layer by the first magnetron sputtering; forming a second transition layer on the surface of the first transition layer by the second magnetron sputtering; forming a color layer on the surface of the second transition layer by the third magnetron sputtering; the second transition layer is a titanium-chromium transition layer. In the second magnetron sputtering, the titanium target is connected to a high-power pulse magnetron sputtering power supply, the power of the high-power pulse magnetron sputtering power supply is 5kW-10kW and the current is 100A-500A; the chromium target is connected to a medium-frequency magnetron sputtering power supply, and the power of the medium-frequency magnetron sputtering power supply is 3kW-12kW. In the preparation method of the wear-resistant and scratch-resistant film, the first transition layer, the second transition layer and the color layer are sequentially formed on the surface of the metal base layer by the magnetron sputtering method. The magnetron sputtering method processes each film layer, which causes less damage to each film layer itself, and the temperature rises slowly during the processing, which is conducive to ensuring the performance of each film layer itself while processing the film. At the same time, by combining medium-frequency magnetron sputtering and high-power pulsed magnetron sputtering, the deposition rate can be increased while the density, hardness, and wear and scratch resistance of the film can be improved. In addition, by processing the titanium-chromium transition layer under different power and current conditions, the stress and element mismatch between the first transition layer and the color layer can be effectively solved, and the bonding strength between the first transition layer, the second transition layer and the color layer can be improved, thereby further improving the wear and scratch resistance of the film.
[0024] The above-mentioned wear-resistant and scratch-resistant film is deposited by combining medium frequency magnetron sputtering + high power pulse magnetron sputtering technologies, which solves the problem of poor film performance such as film density and hardness deposited by medium frequency magnetron sputtering. It also solves the problem of slow deposition rate of pure high power pulse magnetron sputtering. Finally, a wear-resistant and scratch-resistant film with good film density and high nano-hardness is obtained at a relatively low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the structure of the wear-resistant and scratch-resistant film in one embodiment of the present invention.
[0026] Description of the markings in the figure:
[0027] 10. Wear-resistant and scratch-resistant film; 101. Base material; 102. Metal base layer; 103. First transition layer; 104. Second transition layer; 105. Color layer. DETAILED DESCRIPTION
[0028] For ease of understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0030] The chemical formulas "TiCrCN", "TiCrN", "TiN", "CrN", "TiCr", etc. used in this article indicate that the corresponding layer contains the elements listed in the chemical formula, and the ratio between the elements is not limited. For example, the metal base layer is a metal Ti base layer, a metal Cr base layer or a metal TiCr base layer. It shows that the metal base layer can be a metal Ti base layer, a metal Cr base layer or a metal TiCr base layer. When the metal base layer is a metal TiCr base layer, the molar ratio of the Ti element and the Cr element in the metal base layer can be 1:1, or can be a corresponding ratio according to the design.
[0031] For another example, the first transition layer is a TiCrN transition layer, a CrN transition layer or a TiN transition layer. It indicates that: the first transition layer may be a TiCrN transition layer, wherein the molar ratio of the Ti element, the Cr element and the N element in the first transition layer may be 5:9:6, or may be a corresponding designed ratio; the first transition layer may be a CrN transition layer, wherein the molar ratio of the Cr element and the N element in the first transition layer may be 7:3, or may be a corresponding designed ratio; the first transition layer may be a TiN transition layer, wherein the molar ratio of the Ti element and the N element in the first transition layer may be 7:3, or may be a corresponding designed ratio.
[0032] For another example, the second transition layer is a TiCrCN transition layer or a TiCrN transition layer. It is shown that: the second transition layer can be a TiCrCN transition layer, wherein the molar ratio of the Ti element, the Cr element, the C element, and the N element in the second transition layer can be 10:25:1:14, or can be a corresponding ratio according to the design; the second transition layer can be a TiCrN transition layer, wherein the molar ratio of the Ti element, the Cr element, and the N element in the second transition layer can be 2:5:3, or can be a corresponding ratio according to the design.
[0033] For another example, the color layer is a TiCrCN color layer, a TiCrN color layer or a TiN color layer. It indicates that: the color layer can be a TiCrCN color layer, wherein the molar ratio of the Ti element, the Cr element, the C element and the N element in the color layer can be 8:3:1:8, or a corresponding ratio according to the design; the color layer can be a TiCrN color layer, wherein the molar ratio of the Ti element, the Cr element and the N element in the color layer can be 8:3:9, or a corresponding ratio according to the design; the color layer can be a TiN color layer, wherein the molar ratio of the Ti element and the N element in the color layer can be 1:1, or a corresponding ratio according to the design.
[0034] See also Figure 1 An embodiment of the present invention provides a wear-resistant and scratch-resistant film 10, which includes a substrate 101, a metal base layer 102, a first transition layer 103, a second transition layer 104, and a color layer 105. The metal base layer 102 has a bonding surface for bonding to the surface of the substrate 101 and a functional surface arranged opposite to the bonding surface; the first transition layer 103 is located on the functional surface, and the second transition layer 104 is located on the surface of the first transition layer 103 away from the metal base layer 102; the color layer 105 is located on the surface of the second transition layer 104 away from the first transition layer 103. The second transition layer 104 is a titanium-chromium transition layer.
[0035] The wear-resistant and scratch-resistant film 10 in this embodiment has good bonding force between the film layers through the structural design of the metal base layer 102, the first transition layer 103, the second transition layer 104 and the color layer 105, and the film has good wear-resistant and scratch-resistant performance. At the same time, the wear-resistant and scratch-resistant film 10 can show a variety of colors. Specifically, the metal base layer 102 is used as the base layer to provide a stable support for the overall structure of the film. At the same time, the metal base layer 102 can effectively improve the bonding strength between the substrate 101 and the transition layer, so that the film can show stable performance. The arrangement of the first transition layer 103, the second transition layer 104 and the color layer 105 makes the film show the characteristics of compactness and hardness, so that the film shows good wear-resistant and scratch-resistant performance. Further, a titanium-chromium transition layer is arranged between the first transition layer 103 and the color layer 105, which can ensure the stress matching and element matching between the first transition layer 103 and the color layer 105, further enhance the bonding force between the first transition layer 103, the second transition layer 104 and the color layer 105, and further improve the wear-resistant and scratch-resistant performance of the film.
[0036] In a specific example, the thickness ratio of the metal base layer 102, the first transition layer 103, the second transition layer 104 and the color layer 105 is (1-3): (6-10): 1: (3-5). When the thickness of the metal base layer 102, the first transition layer 103, the second transition layer 104 and the color layer 105 is within this ratio, the bonding strength between the layers is the best. As a base layer that can support the overall structure of the film, the metal base layer 102 is difficult to achieve the best manufacturing effect when the thickness ratio between it and other layers is not appropriate. The second transition layer 104 is a transition layer that can match the stress and elements of the first transition layer 103 and the color layer 105. Therefore, in terms of thickness selection, the thickness ratio among the second transition layer 104, the first transition layer 103 and the color layer 105 is particularly important. When the thickness of the second transition layer 104 relative to the first transition layer 103 and the color layer 105 is too small, it is difficult to achieve the effects of stress matching and element matching; when the thickness of the second transition layer 104 relative to the first transition layer 103 and the color layer 105 is too large, on the one hand, the manufacturing cost will be increased, and on the other hand, the second transition layer 104 with too large thickness will lead to stress and element mismatch problems among the first transition layer 103, the second transition layer 104 and the color layer 105, and may even have an adverse effect on the uniformity, integrity and wear and scratch resistance of the film.
[0037] Preferably, the thickness of the second transition layer 104 is 0.05 μm to 0.2 μm. Further preferably, the thickness of the second transition layer 104 is 0.08 μm to 0.15 μm. Specifically, the thickness of the second transition layer 104 can be 0.06 μm, 0.07 μm, 0.1 μm, 0.12 μm, 0.14 μm, 0.16 μm, 0.18 μm, or 0.19 μm.
[0038] As a preferred solution, the thickness of the metal coating layer 102 is 0.1 μm to 0.3 μm, such as 0.12 μm, 0.15 μm, 0.2 μm, 0.24 μm, 0.25 μm, 0.28 μm. The thickness of the first transition layer 103 is 0.6 μm to 1 μm, such as 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm. The thickness of the color layer 105 is 0.3 μm to 0.5 μm, such as 0.32 μm, 0.35 μm, 0.38 μm, 0.4 μm, 0.45 μm, 0.48 μm.
[0039] In a specific example, the thickness of the metal base layer 102 is 0.2 μm, the thickness of the first transition layer 103 is 0.8 μm, the thickness of the second transition layer 104 is 0.1 μm, and the thickness of the color layer 105 is 0.4 μm.
[0040] In a specific example, the substrate is a metal substrate, a ceramic substrate, a glass substrate or a plastic substrate. For example, the metal substrate can be but is not limited to a stainless steel substrate.
[0041] In a specific example, the metal base layer 102 is a metal Ti base layer, a metal Cr base layer or a metal TiCr base layer. The metal Ti base layer, the metal Cr base layer or the metal TiCr base layer can provide a stable support for the overall structure of the film, which is beneficial to improve the stability of the film.
[0042] In a specific example, the first transition layer 103 is a TiCrN transition layer, a CrN transition layer or a TiN transition layer. The second transition layer 104 is a TiCrCN transition layer or a TiCrN transition layer. The color layer 105 is a TiCrCN color layer, a TiCrN color layer or a TiN color layer. In this case, the second transition layer 104 can better ensure the stress matching and element matching between the first transition layer 103 and the color layer 105, better improve the bonding force between the first transition layer 103, the second transition layer 104 and the color layer 105, and better improve the wear resistance and scratch resistance of the film. The color layer 105 is a TiCrCN color layer, a TiCrN color layer or a TiN color layer, which can make the film show a variety of colors. When the color layer 105 is a TiCrCN color layer, a TiCrN color layer or a TiN color layer, the film can show a uniform gold color, and a gold-like film can be obtained. Gold-based films are more popular with customers and the market because of their noble and bright color appearance, but the cost of gold is very high. When the color layer 105 is a TiCrCN color layer, a TiCrN color layer or a TiN color layer, the film can show a uniform gold color, and a gold-like film can be obtained, which can effectively reduce the processing cost of the gold film.
[0043] Another embodiment of the present invention provides a method for preparing a wear-resistant and scratch-resistant film 10, and the method for preparing the wear-resistant and scratch-resistant film 10 comprises the following steps:
[0044] A metal base layer 102 is formed on a substrate 101; a first transition layer 103 is formed on the surface of the metal base layer 102 by a first magnetron sputtering; a second transition layer 104 is formed on the surface of the first transition layer 103 by a second magnetron sputtering; and a color layer 105 is formed on the surface of the second transition layer 104 by a third magnetron sputtering. The second transition layer 104 is a titanium-chromium transition layer. In the second magnetron sputtering, the titanium target is connected to a high-power pulse magnetron sputtering power supply, the power of the high-power pulse magnetron sputtering power supply is 5kW to 10kW and the current is 100A to 500A; the chromium target is connected to a medium-frequency magnetron sputtering power supply, the power of the medium-frequency magnetron sputtering power supply is 3kW to 12kW. When processing the second transition layer 104, by combining medium-frequency magnetron sputtering and high-frequency magnetron sputtering, the deposition rate can be increased while the wear and scratch resistance of the film can be improved. In addition, by processing the titanium-chromium transition layer under different power and current conditions, the stress and element mismatch problems between the first transition layer 103 and the color layer 105 can be effectively solved, and the bonding strength between the first transition layer 103, the second transition layer 104 and the color layer 105 can be improved, thereby further improving the wear resistance and scratch resistance of the film.
[0045] It is understood that during the processing, argon gas can be used as the working gas, and when carbon element needs to be introduced into the second transition layer 104, acetylene can be used as the reaction gas; when nitrogen element needs to be introduced into the second transition layer 104, nitrogen can be used as the reaction gas. The thickness of the second transition layer 104 is controlled by controlling the magnetron sputtering time.
[0046] In a specific example, the first magnetron sputtering uses a medium frequency magnetron sputtering power supply, the power of which is 3kW to 12kW; the third magnetron sputtering uses a high power pulse magnetron sputtering power supply, the power of which is 5kW to 10kW and the current is 100A to 500A. In the process of preparing the thin film, the medium frequency magnetron sputtering power supply is used to process the first transition layer 103 on the surface of the metal base layer 102, and the high power pulse magnetron sputtering power supply is used to process the color layer 105 on the surface of the second transition layer 104.
[0047] Further, when the first transition layer 103 contains titanium and chromium, the titanium target is magnetron sputtered at a power of 5 kW to 10 kW and a current of 100 A to 500 A, and the chromium target is magnetron sputtered at a power of 0.5 kW to 12 kW. Specifically, the titanium target is processed by a high-power pulsed magnetron sputtering power source, and the chromium target is processed by a medium-frequency magnetron sputtering power source.
[0048] When the color layer 105 contains titanium and chromium, the titanium target is magnetron sputtered at a power of 5 kW to 10 kW and a current of 100 A to 500 A, and the chromium target is magnetron sputtered at a power of 0.5 kW to 2 kW. Specifically, the titanium target is processed by a high-power pulsed magnetron sputtering power source, and the chromium target is processed by a medium-frequency magnetron sputtering power source.
[0049] In a specific example, a medium frequency magnetron sputtering power source is used to form the metal base layer on the substrate, and the power of the medium frequency magnetron sputtering power source is 3 kW to 12 kW.
[0050] In a specific example, the method for preparing the wear-resistant and scratch-resistant film 10 further includes the following steps: pre-treating the substrate 101. The pre-treating method is to clean the substrate 101 to remove dirt, oil stains and other residual foreign matter on the surface of the substrate 101. Then, the cleaned substrate 101 is preheated in a vacuum chamber. Preferably, the background vacuum degree of the vacuum chamber is not higher than 8×10 -3Pa, the preheating temperature is 100°C to 150°C. After preheating, the substrate 101 is subjected to arc target bombardment treatment to activate the surface of the substrate 101 and further remove residual foreign matter on the surface of the substrate 101. The conditions of the arc target bombardment treatment are: argon as the working gas, the flow rate is 200sccm to 800sccm; bias voltage is 200V to 600V (duty cycle is 20% to 80%); arc current is 40A to 100A; treatment time is 3min to 10min.
[0051] Another embodiment of the present invention provides a cover plate, which includes a cover plate substrate and the above-mentioned wear-resistant and scratch-resistant film 10 or the wear-resistant and scratch-resistant film 10 prepared by the above-mentioned preparation method. In the structural design of the cover plate, the substrate 101 of the film is located on the surface of the cover plate substrate. The cover plate exhibits good wear resistance and scratch resistance and the performance of presenting various colors, and has good decorative performance.
[0052] Specifically, the cover substrate is a glass cover substrate, a metal cover substrate, a ceramic cover substrate or a plastic cover substrate. By selecting the cover substrate, a variety of cover plates of different materials can be obtained. For example, the cover substrate can be but is not limited to a stainless steel cover substrate.
[0053] Another embodiment of the present invention provides an electronic device, wherein the film of the electronic device is the above-mentioned wear-resistant and scratch-resistant film 10 or the wear-resistant and scratch-resistant film 10 prepared by the above-mentioned preparation method, and the color layer 105 of the film is close to the outer surface of the electronic device.
[0054] Another embodiment of the present invention provides another electronic device, the cover plate of the electronic device is the above-mentioned cover plate, and the color layer 105 of the cover plate is close to the outer surface of the electronic device.
[0055] The following are specific embodiments.
[0056] Example 1
[0057] In the wear-resistant and scratch-resistant film of this embodiment, the substrate is stainless steel; the metal base layer is a metal Cr base layer with a thickness of 0.2 μm; the first transition layer is a CrN transition layer with a thickness of 0.8 μm; the second transition layer is a TiCrCN transition layer with a thickness of 0.1 μm; and the color layer is a TiCrCN color layer with a thickness of 0.4 μm.
[0058] The preparation method of the wear-resistant and scratch-resistant film of this embodiment is:
[0059] S01, cleaning the substrate to remove dirt, oil stains and other residual foreign matter on the surface of the substrate.
[0060] S02, preheat the cleaned substrate in a vacuum chamber, the background vacuum degree of the vacuum chamber is 8.0×10 -3 Pa, preheating temperature is 120℃.
[0061] S03, arc target bombardment treatment is performed on the substrate, argon is used as the working gas, the flow rate is 700 sccm; bias voltage is 500 V (duty cycle is 80%); arc current is 80 A; treatment time is 6 min.
[0062] S04, depositing a metal Cr base layer on the surface of the substrate, the Cr target is connected to a medium frequency magnetron sputtering power supply, argon is used as the working gas, the argon flow rate is 500sccm; the bias voltage is 300V (duty cycle 50%); the Cr target power is 10kW; the thickness of the metal Cr base layer is controlled to be 0.2μm.
[0063] S05, depositing the first transition layer on the surface of the metal Cr base layer, the Cr target is connected to a medium-frequency magnetron sputtering power supply, argon is used as the working gas, and the argon flow rate is 500sccm; the reaction gas is nitrogen, and the nitrogen flow rate is 120sccm; the bias voltage is 200V (duty cycle 50%); the Cr target power is 10kW; and the thickness of the first transition layer is controlled to be 0.8μm.
[0064] S06, depositing the second transition layer on the surface of the first transition layer, the Cr target is connected to a medium-frequency magnetron sputtering power supply, and the Ti target is connected to a high-power pulsed magnetron sputtering power supply; argon is used as the working gas, and the flow rate of argon is 500sccm; the reaction gases are acetylene and nitrogen, the flow rate of acetylene is 20sccm, and the flow rate of nitrogen is 120sccm; the bias voltage is 100V (duty cycle 50%); the Cr target power is 8kW; the Ti target power is 9kW, and the current is 300A; the thickness of the second transition layer is controlled to 0.1μm.
[0065] S07, depositing a color layer on the surface of the second transition layer, the Cr target is connected to a medium frequency magnetron sputtering power supply, the Ti target is connected to a high power pulse magnetron sputtering power supply; argon is used as the working gas, the flow rate of argon is 500sccm; the reaction gases are acetylene and nitrogen, the flow rate of acetylene is 20sccm, and the flow rate of nitrogen is 120sccm; the bias voltage is 100V (duty cycle 50%); the Cr target power is 1.5kW; the Ti target power is 9kW, and the current is 300A; the thickness of the color layer is controlled to be 0.4μm. The wear-resistant and scratch-resistant film in this embodiment is obtained.
[0066] Example 2
[0067] Compared with the embodiment 1, the difference of this embodiment is that the second transition layer is a TiCrN transition layer, and the color layer is a TiCrN color layer.
[0068] The preparation method of the wear-resistant and scratch-resistant film in this embodiment is:
[0069] S01~S05 are the same as in Example 1.
[0070] S06, depositing the second transition layer on the surface of the first transition layer, the Cr target is connected to a medium-frequency magnetron sputtering power supply, and the Ti target is connected to a high-power pulsed magnetron sputtering power supply; argon is used as the working gas, and the flow rate of argon is 50sccm; the reaction gas is nitrogen, and the flow rate of nitrogen is 120sccm; the bias voltage is 100V (duty cycle 50%); the Cr target power is 8kW; the Ti target power is 9kW, and the current is 300A; the thickness of the second transition layer is controlled to 0.1μm.
[0071] S07, depositing a color layer on the surface of the second transition layer, the Cr target is connected to a medium frequency magnetron sputtering power supply, the Ti target is connected to a high power pulse magnetron sputtering power supply; argon is used as the working gas, the flow rate of argon is 500sccm; the reaction gas is nitrogen, the flow rate of nitrogen is 120sccm; the bias voltage is 100V (duty cycle 50%); the Cr target power is 1kW; the Ti target power is 9kW, and the current is 300A; the thickness of the color layer is controlled to be 0.4μm. The wear-resistant and scratch-resistant film in this embodiment is obtained.
[0072] Example 3
[0073] Compared with the embodiment 2, the difference of this embodiment is that the color layer is a TiN color layer.
[0074] The preparation method of the wear-resistant and scratch-resistant film in this embodiment is:
[0075] S01~S06 are the same as those in Example 2.
[0076] S07, depositing a color layer on the surface of the second transition layer, the Ti target is connected to a high-power pulsed magnetron sputtering power supply; using argon as the working gas, the flow rate of argon is 500 sccm; the reaction gas is nitrogen, the flow rate of nitrogen is 100 sccm; the bias voltage is 100 V (duty cycle 50%); the thickness of the color layer is controlled to be 0.4 μm. The wear-resistant and scratch-resistant film in this embodiment is obtained.
[0077] Comparative Example 1
[0078] The wear-resistant and scratch-resistant film of Comparative Example 1 does not contain a second transition layer.
[0079] S01 to S04 are the same as in Example 1
[0080] S05, a transition layer is deposited on the surface of the metal Cr base layer. The Cr target is connected to a medium-frequency magnetron sputtering power supply, and argon is used as the working gas with a flow rate of 500sccm; the reaction gas is nitrogen, and the nitrogen flow rate is 120sccm; the bias voltage is 200V (duty cycle 50%); the Cr target power is 10kW; and the thickness of the first transition layer is controlled to be 0.9μm.
[0081] S06, depositing a color layer on the surface of the transition layer, the Cr target is connected to a medium frequency magnetron sputtering power supply, the Ti target is connected to a medium frequency magnetron sputtering power supply; argon is used as the working gas, the flow rate of argon is 500sccm; the reaction gases are acetylene and nitrogen, the flow rate of acetylene is 26sccm, and the flow rate of nitrogen is 150sccm; the bias voltage is 100V (duty cycle 50%); the Cr target power is 1.8kW; the Ti target power is 6kW; the thickness of the color layer is controlled to be 0.4μm. The wear-resistant and scratch-resistant film in this comparative example is obtained.
[0082] Test Case
[0083] The wear-resistant and scratch-resistant films obtained in Examples 1 to 3 and the film in Comparative Example 1 were subjected to color value detection, nanohardness detection, and wear resistance test.
[0084] Color value detection: L, a, and b in the color value are color values represented by the CIELab color system, and the L value indicates lightness and darkness; the L value range is 0 to 100, and the larger the value, the higher the lightness; the a value range is -128 to 128, representing the saturation of the color on the green-red axis, negative values indicate green, positive values indicate red, and the larger the a value, the redder the color; the b value range is -128 to 128, representing the saturation of the color on the blue-yellow axis, negative values indicate blue, positive values indicate yellow, and the larger the b value, the yellower the color. The film color values L, a, and b are tested by a spectrophotometer using the F2 light source of the CM-3700A-U instrument from Koncia.
[0085] Nanohardness test: The test was carried out using the Anton Paar NHT2 nanohardness tester with a load of 6mN.
[0086] Wear resistance test: Taber 5750 linear friction tester was used for testing with a load of 1000g.
[0087] The test results of color value, nanohardness and wear resistance of the films of Examples 1 to 3 and the film of Comparative Example 1 are shown in the following table.
[0088] Color value detection Nanohardness Wear resistance Example 1 L:75.2, a:2.1, b:18.5 25GPa 2000 cycles Example 2 L:77.8, a:0.5, b:13.5 24.3GPa 2000 cycles Example 3 L:80.5, a:0.8, b:36.5 22.5GPa 2000 cycles Comparative Example 1 L:74.1, a:2.0, b:18.1 17GPa 200 cycles
[0089] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0090] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A wear-resistant and scratch-resistant film, characterized in that: It comprises a substrate, a metal base layer, a first transition layer, a second transition layer and a color layer; the thickness ratio of the metal base layer, the first transition layer, the second transition layer and the color layer is (1-3):(6-10):1:(3-5); The metal primer layer has a bonding surface for bonding to the surface of the substrate and a functional surface arranged opposite to the bonding surface; the first transition layer is located on the functional surface, and the second transition layer is located on the surface of the first transition layer away from the metal primer layer; the color layer is located on the surface of the second transition layer away from the first transition layer; The second transition layer is a titanium-chromium transition layer; The first transition layer is a TiCrN transition layer or a TiN transition layer. When the first transition layer is a TiCrN transition layer, the molar ratio of the Ti element, the Cr element, and the N element is 5:9:6; when the first transition layer is a TiN transition layer, the molar ratio of the Ti element to the N element is 7:3; The second transition layer is a TiCrCN transition layer or a TiCrN transition layer. When the second transition layer is a TiCrCN transition layer, the molar ratio of the Ti element, the Cr element, the C element, and the N element is 10:25:1:14; when the second transition layer is a TiCrN transition layer, the molar ratio of the Ti element, the Cr element, and the N element is 2:5:3; The color layer is a TiCrCN color layer, a TiCrN color layer or a TiN color layer; when the color layer is a TiCrCN color layer, the molar ratio of the Ti element, the Cr element, the C element and the N element is 8:3:1:8; when the color layer is a TiCrN color layer, the molar ratio of the Ti element, the Cr element and the N element is 8:3:9; when the color layer is a TiN color layer, the molar ratio of the Ti element and the N element is 1:
1.
2. The wear-resistant and scratch-resistant film according to claim 1, characterized in that: The thickness of the second transition layer is 0.05 μm-0.2 μm.
3. The wear-resistant and scratch-resistant film according to any one of claims 1 to 2, characterized in that: The metal base layer is a metal Ti base layer, a metal Cr base layer or a metal TiCr base layer.
4. A method for preparing a wear-resistant and scratch-resistant film, characterized in that: The steps include: A metal base layer is formed on a substrate; a first transition layer is formed on the surface of the metal base layer by a first magnetron sputtering; a second transition layer is formed on the surface of the first transition layer by a second magnetron sputtering; a color layer is formed on the surface of the second transition layer by a third magnetron sputtering; the thickness ratio of the metal base layer, the first transition layer, the second transition layer and the color layer is (1-3):(6-10):1:(3-5); The second transition layer is a titanium-chromium transition layer; In the second magnetron sputtering, the titanium target is connected to a high-power pulsed magnetron sputtering power supply, the power of the high-power pulsed magnetron sputtering power supply is 5kW~10kW, and the current is 100A~500A, and the chromium target is connected to a medium-frequency magnetron sputtering power supply, and the power of the medium-frequency magnetron sputtering power supply is 3kW~12kW; The first transition layer is a TiCrN transition layer or a TiN transition layer. When the first transition layer is a TiCrN transition layer, the molar ratio of the Ti element, the Cr element, and the N element is 5:9:6; when the first transition layer is a TiN transition layer, the molar ratio of the Ti element to the N element is 7:3; The second transition layer is a TiCrCN transition layer or a TiCrN transition layer. When the second transition layer is a TiCrCN transition layer, the molar ratio of the Ti element, the Cr element, the C element, and the N element is 10:25:1:14; when the second transition layer is a TiCrN transition layer, the molar ratio of the Ti element, the Cr element, and the N element is 2:5:3; The color layer is a TiCrCN color layer, a TiCrN color layer or a TiN color layer; when the color layer is a TiCrCN color layer, the molar ratio of the Ti element, the Cr element, the C element and the N element is 8:3:1:8; when the color layer is a TiCrN color layer, the molar ratio of the Ti element, the Cr element and the N element is 8:3:9; when the color layer is a TiN color layer, the molar ratio of the Ti element and the N element is 1:
1.
5. The method for preparing the wear-resistant and scratch-resistant film according to claim 4, characterized in that: The first magnetron sputtering adopts a medium frequency magnetron sputtering power supply, and the power of the medium frequency magnetron sputtering power supply is 3kW~12kW; the third magnetron sputtering adopts a high power pulse magnetron sputtering power supply, and the power of the high power pulse magnetron sputtering power supply is 5kW~10kW and the current is 100A~500A.
6. The method for preparing the wear-resistant and scratch-resistant film according to claim 4, characterized in that: When the first transition layer contains titanium and chromium, the titanium target is magnetron sputtered at a power of 5 kW to 10 kW and a current of 100 A to 500 A, and the chromium target is magnetron sputtered at a power of 0.5 kW to 12 kW. When the color layer contains titanium and chromium elements, the titanium target is magnetron sputtered at a power of 5kW~10kW and a current of 100A~500A, and the chromium target is magnetron sputtered at a power of 0.5kW~2kW.
7. The method for preparing the wear-resistant and scratch-resistant film according to any one of claims 4 to 6, characterized in that: The metal base layer is formed on the substrate by using a medium frequency magnetron sputtering power supply, and the power of the medium frequency magnetron sputtering power supply is 3kW-12kW.