A high-efficiency integrated inductor manufacturing process and molding die

By using special powders with low resin solid content and high-efficiency molding, the powders are directly hot-pressed and molded, which solves the problems of cold press damage and long hot pressing time in the prior art, and achieves high-efficiency integrated inductance manufacturing.

CN111599586BActive Publication Date: 2024-11-05HUNAN JINFEILAI ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010535720.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-12
Publication Date
2024-11-05
Estimated Expiration
2040-06-12

AI Technical Summary

Technical Problem

The existing integrated inductor manufacturing process has problems of high defect rate and low production efficiency. The cold pressing step is prone to damage the coil, and the hot pressing process is long, which limits the improvement of production efficiency.

Method used

Using special powder with low resin solid content and efficient mold design, the loose powder is directly heated and shaped and hot-pressed to cure it, reduce cold pressing steps, improve the flowability and heat curing speed of the powder, and shorten the molding. time.

Benefits of technology

It improves yield and production efficiency, shortens the forming time, and the entire process can be completed in as fast as more than 20 seconds, improving product quality and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111599586B_ABST
    Figure CN111599586B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-efficiency integrated inductor manufacturing process: 1) prepare powder, use water-based resin and other components and apply alcohol solution below 75%, add soft magnetic material powder and then disperse and coat with zirconium beads to obtain high-performance powder with low resin content; 2) prepare coil parts, the coil parts include coils; 3) prepare forming molds, the forming molds include upper molds, cover plates, middle molds and bottom molds; 4) place the coil parts on the convex mold part of the middle mold, and then the concave mold part of the cover plate and the convex mold part of the middle mold are molded together; 5) after the convex mold part of the middle mold and the concave mold part of the cover plate are molded together, the powder is fed from the powder feeding hole of the cover plate, so that the set amount of powder required for pressing enters the forming cavity; 6) after the powder feeding is completed, the powder in the forming cavity is hot-pressed by the cooperation of the upper mold and the bottom mold, and after the set pressing time is reached, the mold is removed to take out the integrated inductor. The present invention also discloses a forming mold for implementing the above process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an integrated inductor manufacturing process, and in particular to a high-efficiency integrated inductor manufacturing process and a molding die. Background Art

[0002] The current integrated inductor manufacturing process is to first pre-form and cold-press the powder (also known as iron powder or iron powder) and the coil assembly through a cold forming mold to form a spare inductor semi-finished product; then place the inductor semi-finished product into a hot forming mold for hot pressing, and after the softening, curing, and pressure holding process, an integrated inductor is formed. Chinese invention patent application "Integrated Inductor Forming Method", application number 201811022929.9, application publication number CN109166717A, application publication date 2019-01-08, discloses an integrated inductor forming method: Step 1, place the coil, SMD pins, and iron powder mixed with thermosetting adhesive and coupling agent in the mold cavity of the cold forming mold, and pre-form and cold press at a pressure of 1.8 to 2.5 T / cm2. The coil is fixed in the iron powder and pressed into a semi-finished product. Finished product; Step 2, the thermoforming mold is heated to the preheating temperature, the preheating temperature is higher than the softening temperature that softens the thermosetting binder and facilitates the relative displacement of the iron powder particles; Step 3, the semi-finished product is placed in the inductor accommodating hole and SMD pin accommodating hole provided in the thermoforming mold and heated to the softening temperature; Step 3, the semi-finished product placed in the inductor accommodating hole and SMD pin accommodating hole is hot-pressed with a thermosetting pressure, and the temperature is raised to the thermosetting temperature of the thermosetting binder to solidify the thermosetting binder and maintain the pressure to complete the one-piece molded inductor molding. The above-mentioned one-piece molded inductor molding method adopts the currently more common method of first cold-pressing the coil and powder into an inductor semi-finished product and then hot-pressing it into an integrated inductor. The current integrated inductor manufacturing process has two major shortcomings: First, the defect rate is high because of the cold pressing step. Since the coil is relatively fragile, it is easy to damage the coil during the cold pressing prefabrication of the coil and iron powder, resulting in defects such as coil deformation and short circuit, which leads to the production of defective products; second, the production efficiency is low, and the low production capacity leads to high costs. Although the above-mentioned "Integrated Inductor Forming Method" has added the step of "hot forming mold preheating" to shorten part of the manufacturing time, the entire manufacturing process still takes more than 100 seconds, and because it is first cold pressed and then hot pressed, the inductor after cold pressing is half The finished powder is in a compacted and combined state, so it needs to be softened and reshaped by heating and softening to soften the thermosetting binder and facilitate the relative displacement of the iron powder particles. Therefore, the "heating and softening shaping time" and "heating and pressurizing and curing time" in the hot forming process are relatively long, which must be more than 30 seconds and 50 seconds, which is more than 80 seconds in total. Adding the time of the previous cold pressing step, it will be far more than 100 seconds, which greatly limits the improvement of production efficiency. This is a huge defect brought about by the cold pressing step of the semi-finished inductor, which leads to too long time required for softening and shaping and hot pressing curing. Therefore, there are still many areas that need to be improved and perfected in the current integrated inductor manufacturing process. Summary of the invention

[0003] In view of the above-mentioned deficiencies, the purpose of the present invention is to provide a high-efficiency integrated inductor manufacturing process and molding mold, reduce the steps of cold-pressing the inductor semi-finished products, avoid damage to the coil during the process, increase the yield rate, and at the same time improve production efficiency and product quality.

[0004] The technical solution adopted by the present invention is: a high-efficiency integrated inductor manufacturing process, comprising the following steps:

[0005] 1) Preparation of powder;

[0006] 1.1) Prepare the following components in parts by weight: 15-20 parts of water-based resin; 2-5 parts of amino resin; 1-2 parts of combination aids; 200-300 parts of a mixed solution of water and alcohol, wherein the content of alcohol is controlled to be below 75%; stir and disperse the above components under high-speed conditions of 2500 to 3500 r / min to obtain a resin mixture, and make the solid content of the resin in the resin mixture 0.5% to 1.5%; specifically, the water-based resin is a mixture of one or more of water-based epoxy modified resin, polyester modified resin, and water-based acrylic modified resin; the amino resin is a mixture of one or more of hexamethoxymethyl melamine and methyl etherified high imine melamine; the combination aids include coupling agents, film-forming aids and wetting agents; stir in a high-speed disperser for 25 to 35 minutes to obtain a resin mixture.

[0007] 1.2) The soft magnetic material powder is added to the resin mixture according to the ratio of soft magnetic material powder to resin mixture of 1:0.8 to 1:1.2, and then zirconium beads are added, and the mixture is stirred continuously, first until the liquid is thick, and then until the liquid is completely volatilized into powder, to obtain a powder semi-finished product; during the stirring process, the shear force and friction force of the zirconium beads are used to make the resin mixture with a low resin solid content of 0.5% to 1.5% and the soft magnetic material powder dispersed and coated evenly. Specifically, the mixture is stirred continuously in a planetary mixer, first stirred at high speed until the liquid is thick, then the speed is reduced, and stirred at low speed until the liquid is completely volatilized into powder; wherein, compared with the overall weight of the soft magnetic material powder and the resin mixture, the specific gravity of the zirconium beads added is 5 to 7, and the zirconium beads are high-purity zirconium beads with a diameter of 1 to 5 mm. Among them, the materials used in the inductor, such as ferrite, iron-silicon-aluminum alloy, iron-nickel alloy, etc., can be collectively referred to as soft magnetism, that is, soft magnetic material powder.

[0008] 1.3) The semi-finished powder is baked and screened in turn to obtain the finished powder of the required particle size. Specifically, it is dried in an oven at 90 degrees Celsius for 120 minutes; then screened using a vibrating screening machine, with a screening net of three to five layers, and the mesh size of the gauze is determined according to the required powder size; the powder of each mesh size is screened out and sorted, and after inspection, it is ensured to be dry and free of lumps, and tested using a Hall flow meter, weighing 50g and using a stopwatch to measure the flow rate for 40 to 50 seconds.

[0009] Here, the above powders need to be specifically explained, because the existence of the above powders, relying on their performance, can realize the subsequent process steps. Generally speaking, the higher the purity of the soft magnetic material powder in the powder, the better the performance. The better the performance of the powder, the less copper coil can be used accordingly. That is to say, for the same value of inductance, the higher the purity of the powder, the smaller the volume. The powder prepared by the above process adopts an optimized component formula, a combination of water-based resin and amino resin, and an alcohol solution with a concentration of less than 75%. After adding the soft magnetic material powder, it is dispersed and coated with zirconium beads to achieve high-speed stirring while preventing combustion and explosion. A powder with a uniform coating and a low resin content can be obtained, which improves the performance of the powder and improves the flowability of the powder, so that it can be added from the hole in an hourglass manner. Moreover, due to the uniform resin coating and low content, the subsequent thermal curing time can be reduced, and the quality of the thermal curing effect can be improved. The pressing can make the coating on the surface of each small soft magnetic material powder particle tightly combined. In addition, in the mixed solution of water and alcohol, the alcohol content is controlled below 75%; therefore, during the stirring process, there is no ignition point, and dangers such as combustion and explosion are not likely to occur, thus ensuring production safety.

[0010] In traditional powder preparation, resin + acetone are stirred to disperse the resin. The flash point of acetone is -17.8℃, that is, as long as the temperature is equal to or higher than -17.8℃, the gas volatilized by acetone can burn and cause danger when it encounters a fire source. There are many situations to form a fire source: open flame, electric arc (including electrostatic discharge), sparks generated by impact. In addition, the lower explosion limit of acetone is also very low: 2.6%. The powder is placed in a stirring container, and the dispersed liquid is added appropriately during the stirring process; the stirring process and the precautions for dispersion are the same, so in order to prevent fire and explosion, the stirring process limits the stirring conditions (high-speed stirring is not possible, etc.), and the resin is not easy to cover the powder particles.

[0011] 2) preparing a coil component for use in an integrated inductor, the coil component comprising a coil;

[0012] 3) Preparing a forming mold for an integrated inductor, the forming mold comprising an upper mold, a cover plate, a middle mold and a bottom mold, the upper mold being provided with an upper punch, the bottom mold being provided with a lower punch, the cover plate being provided with an upper punch guide hole, the upper punch guide hole also being used as a powder inlet hole, the middle mold being provided with a lower punch guide hole, the lower side of the cover plate being provided with a die portion, the upper side of the middle mold being provided with a convex mold portion, the convex mold portion being formed with a forming mold cavity and a clamping structure, so that after the coil part is placed in place, the coil corresponds to the forming mold cavity; the die portion and the convex mold portion are adapted to each other, and after the molds are closed, the forming mold cavity corresponds to the upper punch guide hole of the cover plate and the lower punch guide hole of the middle mold respectively;

[0013] 4) Place the coil part on the male part of the middle mold, and then close the female part of the cover plate with the male part of the middle mold so that the coil is located in the molding cavity;

[0014] 5) After the male mold of the middle mold and the female mold of the cover plate are molded together, the powder is fed from the powder feeding hole of the cover plate so that the set amount of powder required for pressing enters the molding cavity;

[0015] 6) After the powder is fed, the upper mold and the bottom mold are used to hot-press the powder in the molding cavity. After the set pressing time is reached, the mold is removed and the integrated inductor is taken out.

[0016] Furthermore, the method further comprises the following steps: 7) performing subsequent heat preservation and shaping on the taken-out integrated inductor.

[0017] It should be noted that in step 2), there are two types of coil parts. One is a coil without a metal frame, that is, a relatively single coil part, including a coil part and a pin part. This type of coil can be placed in the mold by manually placing it one by one, or automatically placed by a special discharge device, or by arranging it through a corresponding discharge mold, so that 10, 20, or 30 coils can be placed at a time. The other type is a coil with a metal frame, that is, the coil sheet described later. In the form of a sheet, multiple coils can be pre-made into sheets for easy placement and mass production. This high-efficiency integrated inductor manufacturing process is applicable to both coil forms.

[0018] It should also be noted that the positioning structure of the male mold part is to fix and position the coil part after it is placed in place; the structure will be slightly different for coils with metal frames and coils without metal frames. For coils without metal frames, the positioning structure of the male mold part only needs to be set for the coil pin part of the coil part; for coils with metal frames (i.e. coil sheets), the positioning structure of the male mold part needs to be set for both the frame part and the coil pin part (pin connection part).

[0019] In step 2), the coil component is a coil sheet, and the coil sheet includes a metal frame and a coil arranged on the metal frame; accordingly, in step 4), the coil component is placed on the male mold part of the middle mold so that the metal frame and the locking structure are in place.

[0020] Furthermore, in step 2), the metal frame is in a strip shape and is arranged with more than two coils; correspondingly, in step 3), the upper die is arranged with more than two upper punches, the bottom die is arranged with more than two lower punches, the cover plate is arranged with more than two upper punch guide holes, and these upper punch guide holes are also used as powder inlet holes, the middle die is arranged with more than two lower punch guide holes, the lower side of the cover plate is arranged with more than two concave die parts, and the upper side of the middle die is arranged with more than two convex die parts.

[0021] Furthermore, in step 2): the strip-shaped metal frame is divided into more than two cells, and pin connection parts are arranged on both sides of each cell; more than two coils are arranged in each cell, and the pins at both ends of each coil are respectively connected to the pin connection parts on both sides of the corresponding cell; in step 3): pin connection part avoidance grooves are arranged on both sides of each male mold part, corresponding to the pin connection parts on both sides of each cell of the metal frame, and correspondingly, avoidance groove pressing groove parts are arranged on both sides of each female mold part; the avoidance groove pressing groove part cooperates with the pin connection part avoidance groove to press and seal the pin connection part.

[0022] Furthermore, in step 3), the upper mold is connected to the upper heating plate of the hot pressing molding equipment, and the bottom mold is connected to the lower heating plate of the hot pressing equipment.

[0023] A high-efficiency integrated inductor forming mold for implementing the process, which is used in conjunction with a coil sheet, the coil sheet comprising a metal frame and a coil arranged on the metal frame; the forming mold comprises an upper mold, a cover plate, a middle mold and a bottom mold, the upper mold is provided with an upper punch, the bottom mold is provided with a lower punch, the cover plate is provided with an upper punch guide hole, the upper punch guide hole is also used as a powder feeding hole, the middle mold is provided with a lower punch guide hole, the lower side of the cover plate is provided with a die portion, the upper side of the middle mold is provided with a convex mold portion, the convex mold portion is formed with a forming mold cavity and a clamping structure, so that after the coil sheet is placed in place, the metal frame corresponds to the clamping structure, the coil corresponds to the forming mold cavity, the die portion is adapted to the convex mold portion, and after the mold is closed, the forming mold cavity corresponds to the upper punch guide hole of the cover plate and the lower punch guide hole of the middle mold respectively.

[0024] Furthermore, the metal frame is strip-shaped and has more than two coils arranged thereon; the upper die is arranged thereon with more than two upper punches, the bottom die is arranged thereon with more than two lower punches, the cover plate is arranged thereon with more than two upper punch guide holes, and these upper punch guide holes are also used as powder inlet holes, the middle die is arranged thereon with more than two lower punch guide holes, the lower side of the cover plate is arranged thereon with more than two concave die parts, and the upper side of the middle die is arranged thereon with more than two convex die parts.

[0025] Furthermore, the strip-shaped metal frame is divided into more than two cells, and pin connection parts are arranged on both sides of each cell; more than two coils are arranged in each cell, and the pins at both ends of each coil are respectively connected to the pin connection parts on both sides of the corresponding cell; pin connection part avoidance grooves are arranged on both sides of each male mold part, corresponding to the pin connection parts on both sides of each cell of the metal frame, and correspondingly, avoidance groove pressing groove parts are arranged on both sides of each female mold part; the avoidance groove pressing groove part cooperates with the pin connection part avoidance groove to press and seal the pin connection part.

[0026] Furthermore, the avoidance groove of the pin connection portion of the male mold portion is a part of the locking structure; the gap portion between two adjacent male mold portions is also a part of the locking structure.

[0027] Furthermore, the pin connection portion is T-shaped, the avoidance groove of the pin connection portion is T-shaped, and the avoidance groove pressing groove portion is also T-shaped.

[0028] The present invention has the following advantages: a high-performance special powder and a corresponding preparation process have been developed, the resin solid content of the powder is low, and the performance is improved while ensuring the fluidity of the powder; the special powder is combined with the use of the cold forming mold to remove the step of pre-forming cold pressing, reduce the use of a set of cold pressing molds, avoid damage to the inductor during the cold pressing forming process, and improve the yield rate; there is no need to cold press the inductor and the powder into a semi-finished inductor, but directly heat and shape the loose powder in a continuous manner, and heat and press solidify the shape, the whole process is very smooth, the powder shaping speed is very fast, and the required holding time is short, the holding shaping can be taken out in advance after about 20 seconds, and then put into the oven for subsequent heat preservation and shaping, so that the molding mold can be quickly vacated for the next manufacturing, and the production efficiency is improved. The entire preparation process can be completed in more than 20 seconds at the fastest, with high efficiency, high yield rate, and better quality.

[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the structure of the coil sheet;

[0031] Figure 2 It is a schematic diagram of the structure of a unit of coil sheet;

[0032] Figure 3 This is a schematic diagram of the structure of the integrated inductor after molding;

[0033] Figure 4 It is a schematic diagram of the structure of a single integrated inductor after forming;

[0034] Figure 5It is a schematic diagram of the overall structure of the forming mold;

[0035] Figure 6 This is a schematic diagram of the front structure of the middle mold;

[0036] Figure 7 for Figure 6 A schematic diagram of a local enlarged structure;

[0037] Figure 8 This is a schematic diagram of the back structure of the middle mold;

[0038] Fig. 9 is a schematic diagram of the structure of the cover plate;

[0039] Fig.10 for Fig. 9 A schematic diagram of a local enlarged structure;

[0040] Fig.11 A schematic diagram of the structure for placing coil sheets;

[0041] Fig.12 It is a schematic diagram of the structure after the coil sheet is placed;

[0042] Fig.13 This is a schematic diagram of the structure after the coil sheet is placed in the middle mold;

[0043] Fig.14 for Fig.13 A schematic diagram of a local enlarged structure;

[0044] Fig.15 It is a schematic diagram of the mold-matching structure of the cover plate and the middle mold;

[0045] Fig.16 A schematic diagram of the structure of a forming mold for hot pressing;

[0046] In the figure: coil sheet 1; metal frame 11; coil 12; pin connection part 13; coil pin 14; upper die 2; upper punch 21; cover plate 3; upper punch guide hole 31; powder feeding hole 31; die portion 32; avoidance groove pressing groove portion 33; middle die 4; lower punch guide hole 41; punch portion 42; forming cavity 43; positioning structure 44; pin connection part avoidance groove 45; bottom die 5; lower punch 51; integrated inductor 6. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, top, bottom, inside, outside, vertical, horizontal, longitudinal, counterclockwise, clockwise, circumferential, radial, axial...), then the directional indication is only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0049] In addition, if there are descriptions involving "first" or "second" etc. in the embodiments of the present invention, the descriptions of "first" or "second" etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0050] Embodiment 1

[0051] See also Figures 1 to 16 The high-efficiency integrated inductor manufacturing process provided in this embodiment includes the following steps:

[0052] 1) Preparation of powder;

[0053] 1.1) Prepare the following components in parts by weight: 15-20 parts of water-based resin; 2-5 parts of amino resin; 1-2 parts of combination aids; 200-300 parts of a mixed solution of water and alcohol, wherein the content of alcohol is controlled to be below 75%; stir and disperse the above components under high-speed conditions of 2500 to 3500 r / min to obtain a resin mixture, and make the solid content of the resin in the resin mixture 0.5% to 1.5%; specifically, the water-based resin is a mixture of one or more of water-based epoxy modified resin, polyester modified resin, and water-based acrylic modified resin; the amino resin is a mixture of one or more of hexamethoxymethyl melamine and methyl etherified high imine melamine; the combination aids include coupling agents, film-forming aids and wetting agents; stir in a high-speed disperser for 25 to 35 minutes to obtain a resin mixture.

[0054] 1.2) Add the soft magnetic material powder to the resin mixture at a ratio of 1:0.8 to 1:1.2, then add zirconium beads, and continue stirring until the liquid is thick, and then stir until the liquid is completely volatilized into powder to obtain a powder semi-finished product; during the stirring process, the shear force and friction of the zirconium beads are used to make the resin mixture with a low resin solid content of 0.5% to 1.5% and the soft magnetic material powder disperse and coat evenly. Specifically, continue stirring in a planetary mixer, first stir at high speed until the liquid is thick, then reduce the speed, and stir at low speed until the liquid is completely volatilized into powder; wherein, compared with the overall weight of the soft magnetic material powder and the resin mixture, the specific gravity of the added zirconium beads is 5 to 7, and the zirconium beads are high-purity zirconium beads with a diameter of 1 to 5 mm.

[0055] 1.3) The semi-finished powder is baked and screened in turn to obtain the finished powder of the required particle size. Specifically, it is dried in an oven at 90 degrees Celsius for 120 minutes; then screened using a vibrating screening machine, with a screening net of three to five layers, and the mesh size of the gauze is determined according to the required powder size; the powder of each mesh size is screened out and sorted, and after inspection, it is ensured to be dry and free of lumps, and tested using a Hall flow meter, weighing 50g and using a stopwatch to measure the flow rate for 40 to 50 seconds.

[0056] 2) See Figures 1 to 2 , a coil component for an integrated inductor is prepared, the coil component is a coil with a metal frame, that is, the coil component is a coil sheet 1, the coil sheet 1 includes a metal frame 11 and a coil 12 arranged on the metal frame 11; wherein the metal frame 11 is in a strip shape, and more than two coils 12 are arranged;

[0057] 3) See Figures 5 to 10 , a forming mold for preparing an integrated inductor, the forming mold comprising an upper mold 2, a cover plate 3, a middle mold 4 and a bottom mold 5, the upper mold 2 is arranged with more than two upper punches 21, the bottom mold 5 is arranged with more than two lower punches 51, the cover plate 3 is arranged with more than two upper punch guide holes 31, and these upper punch guide holes 31 are also used as powder feeding holes 31, the middle mold 4 is arranged with more than two lower punch guide holes 41, the lower side of the cover plate 3 is arranged with more than two concave mold parts 32, and the upper side of the middle mold 4 is arranged with more than two convex mold parts 42; the convex mold part 42 is formed with a forming mold cavity 43 and a clamping structure 44, so that after the coil sheet 1 is placed in place, the metal frame 11 corresponds to the clamping structure 44, the coil 12 corresponds to the forming mold cavity 43, the concave mold part 32 and the convex mold part 42 Correspondingly, after mold closing, the molding cavity 43 corresponds to the upper punch guide hole 31 of the cover plate 3 and the lower punch guide hole 41 of the middle mold 4 respectively; wherein, the upper mold 2 is connected to the upper heating plate of the hot pressing molding equipment, and the bottom mold 5 is connected to the lower heating plate of the hot pressing equipment.

[0058] 4) See Figures 11 to 14 , place the coil sheet 1 on the male part 42 of the middle mold 4 so that the metal frame 11 and the positioning structure 44 are in place, and then the female part 32 of the cover plate 3 and the male part 42 of the middle mold 4 are molded together so that the coil 12 is located in the molding cavity 43.

[0059] 5) See Fig.15 After the male mold part 42 of the middle mold 4 and the female mold part 32 of the cover plate 3 are molded together, the powder is fed from the powder inlet hole 31 of the cover plate, so that the set amount of powder required for pressing enters the molding cavity 33. It should be noted here that the powder can be added manually or a special powder adding device can be designed. It is not the focus of protection required by this application and will not be elaborated here. In addition, it should be noted that the powder should be the special powder prepared as mentioned above. The performance of ordinary powder on the market cannot meet the standards, so its component formula and preparation process are also the focus of protection required by this application. Furthermore, the specific amount of powder added can be adjusted according to the size of the inductor, the density after molding, etc., so it is not specifically limited in this embodiment.

[0060] 6) See Fig.16 After the powder material is fed, the powder material in the molding cavity 33 is hot pressed by the cooperation of the upper mold 2 and the bottom mold 5. After the set pressing time is reached, the mold is removed to take out the integrated inductor 6 (see Figures 3 to 4 ). It should be noted that the heating temperature and pressure control can be adjusted according to the size of the inductor, the density after molding, etc., so they are not specifically limited in this embodiment. For example, the iron powder can be softened and plasticized at a temperature of about 150°C for about 10 seconds, and then the heat curing temperature can be raised to about 170°C, the heat curing pressure can be about 3T / cm2, and the holding time can be about 40 seconds, or the holding time can be about 20 seconds. Then the integrated inductor can be taken out in advance for subsequent heat preservation and shaping, freeing up the molding mold for the next round of processing. In addition, it is also necessary to emphasize that, since a cover plate is designed and a through hole is designed on the cover plate, the through hole is used as an "upper punch guide hole and a powder entry hole" at the same time, so that the powder can be directly added to the molding cavity without the step of cold pressing to form an inductor semi-finished product, that is to say, the powder will not be cold pressed into a certain shape first, and the powder is in a loose and flowing state in the molding cavity and can be quickly heated to soften the plasticity; while the current cold-pressed inductor semi-finished products, since the powder has been cold pressed into a certain shape (primary shaping), the compacted powder in block form must be heated and softened in the molding cavity to soften the thermosetting binder and facilitate the relative displacement of the iron powder particles before shaping (secondary shaping) can be performed, which results in the shaping process taking a long time.

[0061] Specifically, in step 2), the strip-shaped metal frame 11 is divided into more than two cells, and pin connection parts 13 are arranged on both sides of each cell; more than two coils 12 are arranged in each cell, and the pins (coil pins 14) at both ends of each coil 12 are respectively connected to the pin connection parts 13 on both sides of the corresponding cell; correspondingly, in step 3), the two sides of each male mold part 42 are provided with pin connection part avoidance grooves 45, correspondingly, the two sides of each female mold part 32 are provided with avoidance groove pressing groove parts 33; the avoidance groove pressing groove parts 33 cooperate with the pin connection part avoidance grooves 45 to compress and seal the pin connection parts 13. After a whole row of integrated inductors are formed, each integrated inductor needs to be cut off from the pin connection part of the metal frame to obtain a single integrated inductor.

[0062] Here, there are a few points that need to be explained: First, regarding the die portion provided on the cover plate and the punch portion provided on the middle mold, for each coil on the coil sheet, there is a set of corresponding die portions and punch portions to form a corresponding molding cavity; of course, in principle, the positions of the die portion and the punch portion can be swapped, that is, the cover plate is provided with the punch portion, and the middle mold is provided with the die portion, which is also an equivalent layout method, but in order to facilitate the subsequent placement of the coil sheet, it is more reasonable to set the punch portion on the cover plate (located below). Second, regarding the molding cavity and the locking structure formed by the male mold part; those skilled in the art can understand that the molding cavity is formed in the male mold part (the raised part of the male mold part surrounds the molding cavity), but it needs to be used in conjunction with the female mold part to perform the mold closing work; in addition, for the locking structure, its purpose is to position and clamp the coil sheet. When the metal frame of the coil sheet is in the shape of a strip and there are more than two coils arranged (divided into multiple cells), the locking structures on the multiple male mold parts are also coordinated with each other for the structure of the coil sheet. At this time, the avoidance groove of the pin connection part of the male mold part is a part of the locking structure; the gap between two adjacent male mold parts is also a part of the locking structure. Third, regarding the coordination between the upper mold, cover plate, middle mold and bottom mold, for the steps of the above-mentioned high-efficiency integrated inductor manufacturing process, it is obvious that the bottom mold will first cooperate with the middle mold, and the lower punch will be inserted into the lower punch guide hole in place (so that the molding cavity can obtain appropriate space and avoid leakage of powder when adding powder later), and then the cover plate and the middle mold will be molded together, that is, the concave mold part and the convex mold part will be molded together, and then the appropriate amount of powder will be added through the upper punch guide hole, that is, into the powder hole, and finally the upper mold and the cover plate will cooperate, the upper punch will be inserted into the upper punch guide hole, and the upper mold and the bottom mold will cooperate to perform hot pressing on the powder in the molding cavity. Fourth, in order to further shorten the time, the upper mold, cover plate, middle mold or bottom mold can also be preheated.

[0063] See also Figures 1 to 2 , 5 to Fig.10, a high-efficiency integrated inductor forming mold for implementing the process is used in conjunction with a coil sheet 1, wherein the coil sheet 1 includes a metal frame 12 and a coil 12 arranged on the metal frame 11; the forming mold includes an upper mold 2, a cover plate 3, a middle mold 4 and a bottom mold 5, wherein the upper mold 2 is provided with an upper punch 21, the bottom mold 5 is provided with a lower punch 51, the cover plate 3 is provided with an upper punch guide hole 31, and the upper punch guide hole 31 also serves as a powder inlet hole 31 In use, the middle die 4 is provided with a lower punch guide hole 41, the lower side of the cover plate 3 is provided with a die portion 32, and the upper side of the middle die 4 is provided with a convex die portion 42, and the convex die portion 42 is formed with a molding cavity 43 and a clamping structure 44, so that after the coil sheet 1 is placed in place, the metal frame 11 corresponds to the clamping structure 44, the coil 12 corresponds to the molding cavity 43, the die portion 32 is adapted to the convex die portion 42, and after the mold is closed, the molding cavity 43 corresponds to the upper punch guide hole 31 of the cover plate 3 and the lower punch guide hole 41 of the middle die 4 respectively.

[0064] Specifically, the metal frame 1 is strip-shaped and has more than two coils 12 arranged thereon; the upper die 2 is provided with more than two upper punches 21, the bottom die 5 is provided with more than two lower punches 51, the cover plate 3 is provided with more than two upper punch guide holes 31, and these upper punch guide holes 31 are also used as powder inlet holes 31, the middle die 4 is provided with more than two lower punch guide holes 41, the lower side of the cover plate 3 is provided with more than two concave die parts 32, and the upper side of the middle die 4 is provided with more than two convex die parts 42.

[0065] Specifically, the strip-shaped metal frame 11 is divided into more than two cells, and pin connection parts 13 are arranged on both sides of each cell; more than two coils 12 are respectively arranged in each cell, and the pins (coil pins 14) at both ends of each coil are respectively connected to the pin connection parts 13 on both sides of the corresponding cell; pin connection part avoidance grooves 45 are arranged on both sides of each male mold part 42, corresponding to the pin connection parts 13 on both sides of each cell of the metal frame 11, and correspondingly, avoidance groove pressing groove parts 33 are arranged on both sides of each female mold part 32; the avoidance groove pressing groove part 33 cooperates with the pin connection part avoidance groove 45 to compress and seal the pin connection part 13.

[0066] Specifically, the pin connection portion avoidance groove 45 of the male mold portion 42 is a part of the locking structure 44; the gap between two adjacent male mold portions 42 is also a part of the locking structure. Fig.10 ), which helps with positioning, sealing, and improving the quality of the mold closing between the male and female mold parts.

[0067] Specifically, the pin connection portion 13 is T-shaped, the pin connection portion avoidance groove 45 is T-shaped, and the avoidance groove pressing groove portion 33 is also T-shaped. The pin connection portion 13, the pin connection portion avoidance groove 45, and the avoidance groove pressing groove portion 33 adopt a T-shaped matching structural design, which can better perform positioning and compression sealing, ensure the quality of hot pressing molding, and can also be more convenient for welding with the coil pin 14.

[0068] It should be noted here that in step 2), there are two forms of coil parts, one is a coil without a metal frame, that is, a relatively single coil part, including a coil part and a pin part. This type of coil can be placed in the mold by manually placing it one by one, or by automatically placing it through a special discharge device, or by arranging it through a corresponding discharge mold, placing 10, 20, 30 at a time. The other is a coil with a metal frame, that is, the coil sheet, which adopts the form of a sheet, and multiple coils can be pre-made into sheets, which is convenient for placement and batch production. The first embodiment of this invention is an implementation plan for a coil with a metal frame (i.e., a coil sheet); however, this high-efficiency integrated inductor manufacturing process is also applicable to coils without a metal frame. It is only necessary to slightly adjust the structure of the convex mold part on the upper side of the middle mold to adapt to the coil without a metal frame. That is to say, if a coil without a metal frame is used, the structure of the convex part on the upper side of the middle mold can be more concise, and the convex part 42 is formed with a molding cavity 43 and a clamping structure 44, wherein the clamping structure 44 only needs to be set for the pin part of the coil without a metal frame. Therefore, the clamping structure of the convex part in the claims is a high-level concept, through which the coil part is placed in place, and the coil part is fixed and positioned, and its specific structure can be changed for different forms of coil parts, so its description and summary are reasonable.

[0069] Embodiment 2

[0070] This embodiment is basically the same as the first embodiment, except that:

[0071] Preparation of powder;

[0072] 1.1) Prepare the following components by weight: 18 parts of water-based resin; 3 parts of amino resin; 1.5 parts of combination additives; 250 parts of a mixed solution of water and alcohol, wherein the content of alcohol is controlled to be below 75%; stir and disperse the above components at a high speed of 3000r / min to obtain a resin mixture, and make the solid content of the resin in the resin mixture be 1%; specifically, the water-based resin is selected from one or more of ADL-118 water-based epoxy modified resin, AT-580 polyester modified resin, and AT-888 water-based acrylic modified resin produced by Taiwan Uda Resin Chemical, China; the amino resin is a mixture of one or more of CYMEL303 hexamethoxymethyl melamine and CYMEL325 methyl etherified high imine melamine produced by American Cytec; the combination additives include American Dow Corning silane coupling agent 6040 / 6021, Dow Chemical dpnp film-forming additive, tacowet 4000 wetting agent, in this embodiment, the ratio of the three can be adjusted appropriately according to actual conditions; stir in a high-speed disperser for 30 minutes to obtain a resin mixture.

[0073] 1.2) Add the soft magnetic material powder to the resin mixture at a ratio of 1:1, then add zirconium beads, and continue stirring until the liquid is thick, and then stir until the liquid is completely volatilized into powder to obtain a powder semi-finished product; during the stirring process, the shear force and friction of the zirconium beads are used to make the resin mixture with a low resin solid content of 1% and the soft magnetic material powder dispersed and coated evenly. Specifically, continue stirring in a planetary mixer, first stir at high speed until the liquid is thick, then reduce the speed, and stir at low speed until the liquid is completely volatilized into powder; wherein, compared with the overall weight of the soft magnetic material powder and the resin mixture, the specific gravity of the added zirconium beads is 6, and the zirconium beads are high-purity zirconium beads with a diameter of 1 to 5 mm.

[0074] 1.3) The semi-finished powder is baked and screened in turn to obtain the finished powder of the required particle size. Specifically, it is dried in an oven at 90 degrees Celsius for 120 minutes; then screened using a vibrating screening machine, the screening net is three to five layers, and the mesh number of the gauze is determined according to the required powder size. The mesh numbers usually used are 80 / 100 / 150 / 200 / 300 / 500.

[0075] Embodiment 3

[0076] This embodiment is basically the same as the second embodiment, except that:

[0077] Preparation of powder;

[0078] 1.1) Prepare the following components by weight: 15 parts of water-based resin; 2 parts of amino resin; 1 part of combination auxiliary agent; 200 parts of a mixed solution of water and alcohol, wherein the content of alcohol is controlled to be below 75%; stir and disperse the above components at a high speed of 2500r / min to obtain a resin mixture, and make the solid content of the resin in the resin mixture 0.5%; specifically, the water-based resin is selected from ADL-118 water-based epoxy modified resin, AT-580 polyester modified resin, AT-888 water-based acrylic modified resin produced by Taiwan Uda Resin Chemical, China, one or more of which are mixed; the amino resin is a mixture of CYMEL303 hexamethoxymethyl melamine and CYMEL325 methyl etherified high imine melamine produced by American Cytec; the combination auxiliary agent includes American Dow Corning silane coupling agent 6040 / 6021, Dow Chemical dpnp film-forming agent, taco wet 4000 wetting agent, in this embodiment, the ratio of the three can be adjusted appropriately according to actual conditions; stirring in a high-speed disperser for 25 minutes to obtain a resin mixture.

[0079] 1.2) Add the soft magnetic material powder to the resin mixture at a ratio of 1:0.8, then add zirconium beads, and continue stirring until the liquid is thick, and then stir until the liquid is completely volatilized into powder to obtain a powder semi-finished product; during the stirring process, the shear force and friction of the zirconium beads are used to make the resin mixture with a low resin solid content of 0.5% and the soft magnetic material powder disperse and coat evenly. Specifically, continue stirring in a planetary mixer, first stir at high speed until the liquid is thick, then reduce the speed, and stir at low speed until the liquid is completely volatilized into powder; wherein, compared with the overall weight of the soft magnetic material powder and the resin mixture, the specific gravity of the zirconium beads added is 5, and the zirconium beads are high-purity zirconium beads with a diameter of 1 to 5 mm.

[0080] 1.3) The semi-finished powder is baked and screened in turn to obtain the finished powder of the required particle size. Specifically, it is dried in an oven at 90 degrees Celsius for 120 minutes; then screened using a vibrating screening machine, the screening net is three to five layers, and the mesh number of the gauze is determined according to the required powder size. The mesh numbers usually used are 80 / 100 / 150 / 200 / 300 / 500.

[0081] Embodiment 4

[0082] This embodiment is basically the same as the second embodiment, except that:

[0083] Preparation of powder;

[0084] 1.1) Prepare the following components by weight: 20 parts of water-based resin; 5 parts of amino resin; 2 parts of combination additives; 300 parts of a mixed solution of water and alcohol, wherein the content of alcohol is controlled to be below 75%; stir and disperse the above components at a high speed of 3500r / min to obtain a resin mixture, and make the solid content of the resin in the resin mixture be 1.5%; specifically, the water-based resin is selected from one or more of ADL-118 water-based epoxy modified resin, AT-580 polyester modified resin, and AT-888 water-based acrylic modified resin produced by Taiwan Uda Resin Chemical, China; the amino resin is a mixture of one or more of CYMEL303 hexamethoxymethyl melamine and CYMEL325 methyl etherified high imine melamine produced by American Cytec; the combination additives include American Dow Corning silane coupling agent 6040 / 6021, Dow Chemical dpnp film-forming additive, taco wet 4000 wetting agent, in this embodiment, the ratio of the three can be adjusted appropriately according to actual conditions; stirring in a high-speed disperser for 35 minutes to obtain a resin mixture.

[0085] 1.2) Add the soft magnetic material powder to the resin mixture at a ratio of 1:1.2, then add zirconium beads, and continue stirring until the liquid is thick, and then stir until the liquid is completely volatilized into powder to obtain a powder semi-finished product; during the stirring process, the shear force and friction of the zirconium beads are used to make the resin mixture with a low resin solid content of 1.5% and the soft magnetic material powder disperse and coat evenly. Specifically, continue stirring in a planetary mixer, first stir at high speed until the liquid is thick, then reduce the speed, and stir at low speed until the liquid is completely volatilized into powder; wherein, compared with the overall weight of the soft magnetic material powder and the resin mixture, the specific gravity of the zirconium beads added is 7, and the zirconium beads are high-purity zirconium beads with a diameter of 1 to 5 mm.

[0086] 1.3) The semi-finished powder is baked and screened in turn to obtain the finished powder of the required particle size. Specifically, it is dried in an oven at 90 degrees Celsius for 120 minutes; then screened using a vibrating screening machine, the screening net is three to five layers, and the mesh number of the gauze is determined according to the required powder size. The mesh numbers usually used are 80 / 100 / 150 / 200 / 300 / 500.

[0087] The present invention is not limited to the above-mentioned implementation mode. Other high-efficiency integrated inductor manufacturing processes and molding dies obtained by adopting the same or similar technical features as the above-mentioned embodiments of the present invention are within the protection scope of the present invention.

Claims

1. A high-efficiency integrated inductor manufacturing process, characterized in that: The steps include: 1) Preparation of powder; 1.1) Prepare the following components by weight: 15-20 parts of water-based resin; 2-5 parts of amino resin; 1-2 parts of combination auxiliary agent; 200-300 parts of a mixed solution of water and alcohol, wherein the content of alcohol is controlled to be below 75%; stir and disperse the above components at a high speed of 2500 to 3500 r / min to obtain a resin mixture, and make the solid content of the resin in the resin mixture be 0.5% to 1.5%; 1.2) Adding the soft magnetic material powder to the resin mixed liquid at a ratio of 1:0.8 to 1:1.2, and then adding zirconium beads, and continuously stirring, first stirring until the liquid thickens, and then stirring until the liquid completely evaporates into powder, to obtain a powder semi-finished product; during the stirring process, the shear force and friction force of the zirconium beads are used to make the resin mixed liquid with a low resin solid content of 0.5% to 1.5% and the soft magnetic material powder uniformly dispersed and coated; 1.3) The semi-finished powder is baked and screened in sequence to obtain the finished powder of the required particle size; 2) preparing a coil component for use in an integrated inductor, the coil component comprising a coil; 3) Preparing a forming mold for an integrated inductor, the forming mold comprising an upper mold, a cover plate, a middle mold and a bottom mold, the upper mold being provided with an upper punch, the bottom mold being provided with a lower punch, the cover plate being provided with an upper punch guide hole, the upper punch guide hole also being used as a powder inlet hole, the middle mold being provided with a lower punch guide hole, the lower side of the cover plate being provided with a die portion, the upper side of the middle mold being provided with a convex mold portion, the convex mold portion being formed with a forming mold cavity and a clamping structure, so that after the coil part is placed in place, the coil corresponds to the forming mold cavity; the die portion and the convex mold portion are adapted to each other, and after the molds are closed, the forming mold cavity corresponds to the upper punch guide hole of the cover plate and the lower punch guide hole of the middle mold respectively; 4) Place the coil part on the male part of the middle mold, and then close the female part of the cover plate with the male part of the middle mold so that the coil is located in the molding cavity; 5) After the male mold of the middle mold and the female mold of the cover plate are molded together, the powder is fed from the powder feeding hole of the cover plate so that the set amount of powder required for pressing enters the molding cavity; 6) After the powder is fed, the upper mold and the bottom mold are used to hot-press the powder in the molding cavity. After the set pressing time is reached, the mold is removed and the integrated inductor is taken out.

2. The high-efficiency integrated inductor manufacturing process according to claim 1, characterized in that: The method also includes the following steps: 7) performing subsequent heat preservation and shaping on the taken-out integrated inductor.

3. The high-efficiency integrated inductor manufacturing process according to claim 1, characterized in that: In step 1.1), the water-based resin is a mixture of one or more of a water-based epoxy modified resin, a polyester modified resin, and a water-based acrylic modified resin; the amino resin is a mixture of one or more of hexamethoxymethyl melamine and methyl etherified high imine melamine; the combined auxiliary agent includes a coupling agent, a film-forming auxiliary agent and a wetting agent; stirring is performed in a high-speed disperser for 25 to 35 minutes to obtain a resin mixture.

4. The high-efficiency integrated inductor manufacturing process according to claim 1, characterized in that: In step 1.2), continuous stirring is performed in a planetary mixer, first at high speed until the liquid thickens, then the speed is reduced and stirred at low speed until the liquid completely evaporates into powder; wherein, compared with the overall weight of the soft magnetic material powder and the resin mixture, the specific gravity of the zirconium beads added is 5 to 7, and the zirconium beads are high-purity zirconium beads with a diameter of 1 to 5 mm.

5. The high-efficiency integrated inductor manufacturing process according to claim 1, characterized in that: In step 1.3), the powder is dried in an oven at 90 degrees Celsius for 120 minutes. The powder is then screened using a vibrating screening machine with a three- to five-layer screening screen and a mesh size that is determined based on the size of the powder required. The powder of each mesh size is screened out and sorted, and after inspection, it is ensured to be dry and free of lumps. The powder is then tested using a Hall flowmeter, weighing 50 g and measuring the flow rate using a stopwatch for 40 to 50 seconds.

6. The high-efficiency integrated inductor manufacturing process according to claim 1, characterized in that: In step 2), the coil component is a coil sheet, and the coil sheet includes a metal frame and a coil arranged on the metal frame; accordingly, in step 4), the coil component is placed on the male mold part of the middle mold so that the metal frame and the locking structure are in place.

7. The high-efficiency integrated inductor manufacturing process according to claim 6, characterized in that: In step 2), the metal frame is in a strip shape and is arranged with more than two coils; correspondingly, in step 3), the upper die is arranged with more than two upper punches, the bottom die is arranged with more than two lower punches, the cover plate is arranged with more than two upper punch guide holes, and these upper punch guide holes are also used as powder inlet holes, the middle die is arranged with more than two lower punch guide holes, the lower side of the cover plate is arranged with more than two concave die parts, and the upper side of the middle die is arranged with more than two convex die parts.

8. The high-efficiency integrated inductor manufacturing process according to claim 7, characterized in that: In step 2), the strip-shaped metal frame is divided into more than two cells, and pin connection parts are arranged on both sides of each cell; more than two coils are arranged in each cell, and the pins at both ends of each coil are respectively connected to the pin connection parts on both sides of the corresponding cell; in step 3), pin connection part avoidance grooves are arranged on both sides of each male mold part, corresponding to the pin connection parts on both sides of each cell of the metal frame, and correspondingly, avoidance groove pressing groove parts are arranged on both sides of each female mold part; the avoidance groove pressing groove part cooperates with the pin connection part avoidance groove to press and seal the pin connection part.

9. The high-efficiency integrated inductor manufacturing process according to claim 1, characterized in that: In step 3), the upper mold is connected to the upper heating plate of the hot pressing molding equipment, and the bottom mold is connected to the lower heating plate of the hot pressing equipment.

10. A high-efficiency integrated inductor forming mold for implementing the process described in any one of claims 1 to 9, characterized in that: It includes an upper die, a cover plate, a middle die and a bottom die, the upper die is provided with an upper punch, the bottom die is provided with a lower punch, the cover plate is provided with an upper punch guide hole, the upper punch guide hole is also used as a powder inlet hole, the middle die is provided with a lower punch guide hole, the lower side of the cover plate is provided with a die portion, the upper side of the middle die is provided with a punch portion, the punch portion is formed with a molding cavity and a clamping structure, the die portion is adapted to the punch portion, and after mold closing, the molding cavity corresponds to the upper punch guide hole of the cover plate and the lower punch guide hole of the middle die respectively.

11. The high-efficiency integrated inductor forming mold according to claim 10, characterized in that: The upper die is arranged with more than two upper punches, the bottom die is arranged with more than two lower punches, the cover plate is arranged with more than two upper punch guide holes, and these upper punch guide holes are also used as powder inlet holes, the middle die is arranged with more than two lower punch guide holes, the lower side of the cover plate is arranged with more than two concave die parts, and the upper side of the middle die is arranged with more than two convex die parts.

12. The high-efficiency integrated inductor forming mold according to claim 11, characterized in that: Pin connection portion avoidance grooves are arranged on both sides of each die portion, and correspondingly, avoidance groove pressing groove portions are arranged on both sides of each die portion.

13. The high-efficiency integrated inductor forming mold according to claim 12, characterized in that: The avoidance groove of the pin connection part of the male mold part is a part of the locking structure; the gap part between two adjacent male mold parts is also a part of the locking structure.