Method for manufacturing semiconductor element
In semiconductor component manufacturing, the bonding method of nitride semiconductor layer and specific wafer surface structure design is used to solve the problem of cracks in semiconductor layer, productivity and yield are improved, and process stability is achieved.
Patent Information
- Application Number
- CN202010131962.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-04
- Filing Date
- 2020-02-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-02-28
AI Technical Summary
In the process of semiconductor component manufacturing, the crack problem of semiconductor layer leads to a decrease in productivity, which is difficult to effectively solve in the prior art.
By forming a nitride semiconductor layer on the first wafer and designing a specific wafer surface structure, the second wafer is bonded to the semiconductor layer, and the step portion and the inclined portion are used to prevent the thick film portion from contacting the second wafer. The second wafer is stably fixed as a support substrate.
The crack density in the semiconductor layer is effectively reduced, the yield and productivity are improved, and the stability of the process is ensured.
Smart Images

Figure CN111628054B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor element. Background Art
[0002] As one of the methods for manufacturing semiconductor elements such as light emitting diodes (LEDs), for example, Patent Document 1 discloses a method of growing a semiconductor layer on a growth substrate such as a sapphire substrate, i.e., a wafer, and then bonding it to a support substrate. In such a method for manufacturing semiconductor elements, cracks may occur in the semiconductor layer, which may reduce productivity.
[0003] Patent Document 1: International Publication No. 2011 / 161975 Summary of the invention
[0004] Technical problem to be solved by the invention
[0005] One embodiment of the present invention has been made in view of the above-mentioned technical problems, and an object of the present invention is to provide a method for manufacturing a semiconductor element that can improve productivity.
[0006] Technical solutions for solving technical problems
[0007] A method for manufacturing a semiconductor element according to an embodiment of the present invention comprises: a step of forming a semiconductor layer composed of a nitride semiconductor on a first wafer; and a step of bonding a second wafer to the first wafer via the semiconductor layer. The upper surface of the first wafer includes a first region and a second region, the second region being arranged around the first region and being located at a lower position than the first region. When the first wafer is viewed from above, a first distance between the end edge of the first wafer and the first region in a first direction passing through the center of the first wafer and parallel to the m-axis of the semiconductor layer is shorter than a second distance between the end edge of the first wafer and the first region in a second direction passing through the center of the first wafer and parallel to the a-axis of the semiconductor layer. The lower surface of the second wafer includes a flat portion and an inclined portion, the inclined portion being arranged around the flat portion and inclined from the flat portion toward the upper surface. In the step of bonding the second wafer, the end of the first wafer located in the first direction is bonded to the inclined portion of the second wafer so as to face each other.
[0008] Effects of the Invention
[0009] According to one embodiment of the present invention, a method for manufacturing a semiconductor element capable of improving productivity can be realized. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1This is a flowchart showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.
[0011] Figure 2A FIG. 1 is a top view showing a first wafer according to an embodiment of the present invention.
[0012] Figure 2B It is along Figure 2A A partial cross-sectional view in the first direction shown.
[0013] Figure 2C It is along Figure 2A A partial cross-sectional view in the second direction shown.
[0014] Figure 3A FIG. 1 is a plan view showing a first wafer and a semiconductor layer in an embodiment.
[0015] Figure 3B It is along Figure 3A A partial cross-sectional view in the first direction shown.
[0016] Figure 3C It is along Figure 3A A partial cross-sectional view in the second direction shown.
[0017] Figure 4A It is a top view showing the crystal orientation of the semiconductor layer.
[0018] Figure 4B It is a three-dimensional diagram showing the crystal orientation of the semiconductor layer.
[0019] Figure 5 FIG. 1 is a bottom view showing a second wafer according to an embodiment of the present invention.
[0020] Fig. 6A FIG. 1 is a plan view showing a first wafer, a semiconductor layer, and a second wafer according to an embodiment of the present invention.
[0021] Figure 6B It is along Fig. 6A A partial cross-sectional view in the first direction shown.
[0022] Figure 6C It is along Fig. 6A A partial cross-sectional view in the second direction shown.
[0023] Fig. 7A It is a top view showing a method for manufacturing a semiconductor element according to a comparative example.
[0024] Figure 7B It is a partial cross-sectional view showing a method for manufacturing a semiconductor element according to a comparative example.
[0025] Fig. 8AIt is a top view showing a method for manufacturing a semiconductor element according to a reference example.
[0026] Figure 8B It is a partial cross-sectional view showing a method for manufacturing a semiconductor element according to a reference example.
[0027] Fig.9A FIG. 1 is a plan view showing the first wafer and the semiconductor layer in the experimental example.
[0028] Fig. 9B The horizontal axis is the radial position and the vertical axis is the height of the upper surface of the semiconductor layer. Fig.9A A graph showing the shape of the semiconductor layer along line segment AA'.
[0029] Fig. 9C The horizontal axis is the angle θ, and the vertical axis is the protrusion H. Fig.9A Circle B is a graph of the shape of the semiconductor layer.
[0030] Description of Reference Numerals
[0031] 10: first wafer; 11: first region; 12: second region; 13: rounded portion; 14: extension portion; 15: upper surface; 16: step portion; 17: end edge; 18: bevel portion; 19: orientation plane; 20: semiconductor layer; 20a: thick film portion; 30: second wafer; 31: lower surface; 32: flat portion; 33: inclined portion; 35: upper surface; 36: flat portion; 37: inclined portion; 110: first wafer; 115: upper surface; 1 20: semiconductor layer; 120a: thick film portion; 121: crack; 210: first wafer; 211: first region; 212: second region; 215: upper surface; 216: step portion; 220: semiconductor layer; 220a: thick film portion; C: center of the first wafer; D1: first distance; D2: second distance; G: height of step portion 16; H: protrusion; V1: first direction; V2: second direction; t1, t2: film thickness; θ: angle. DETAILED DESCRIPTION
[0032] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings. It should be noted that each figure is schematic or conceptual, and emphasis and omission are appropriately made to make the drawings easier to observe. The shapes and dimensional ratios of the parts shown in the figures are not necessarily the same as in reality. There are also cases where the dimensional ratios and shapes of the parts are not strictly consistent between the drawings. In the following description, the same figure marks are marked for the components that have appeared, and detailed descriptions are omitted.
[0033] First, a method for manufacturing a semiconductor device according to an embodiment of the present invention will be briefly described.
[0034] The method for manufacturing a semiconductor device of the present embodiment includes a step of forming a semiconductor layer 20 made of a nitride semiconductor on a first wafer 10 (step S2 ) and a step of bonding a second wafer 30 to the first wafer 10 via the semiconductor layer 20 (step S3 ).
[0035] The upper surface 15 of the first wafer 10 includes a first region 11 and a second region 12, the second region 12 being arranged around the first region 11 and being located at a lower position than the first region 11. When the first wafer 10 is viewed from above, a first distance D1 between the end edge 17 of the first wafer 10 and the first region 11 in a first direction V1 passing through the center of the first wafer 10 and parallel to the m-axis of the semiconductor layer 20 is shorter than a second distance D2 between the end edge 17 of the first wafer 10 and the first region 11 in a second direction V2 passing through the center of the first wafer 10 and parallel to the a-axis of the semiconductor layer 20. The lower surface 31 of the second wafer 30 includes a flat portion 32 and an inclined portion 33, the inclined portion 33 being arranged around the flat portion 32 and inclined from the flat portion toward the upper surface 35 of the second wafer 30. In the process of bonding the second wafer 30, the end of the first wafer 10 located in the first direction V1 is made to face the inclined portion 33 of the second wafer 30 and bonded.
[0036] Hereinafter, the method for manufacturing the semiconductor element according to the present embodiment will be described in detail.
[0037] Figure 1 This is a flowchart showing the method for manufacturing a semiconductor element according to the present embodiment.
[0038] (Step of Preparing First Wafer 10)
[0039] First, if Figure 1 As shown in step S1 , a first wafer 10 is prepared.
[0040] Figure 2A 1 is a plan view showing the first wafer 10 according to the present embodiment.
[0041] Figure 2B It is along Figure 2A A partial cross-sectional view in the first direction V1 is shown.
[0042] Figure 2C It is along Figure 2A A partial cross-sectional view in the second direction V2 is shown.
[0043] The first wafer 10 is, for example, a sapphire substrate, for example, made of single crystal sapphire. Figure 2A As shown, the first wafer 10 is roughly disc-shaped, with a diameter of, for example, about 100 mm. A chord-shaped orientation plane 19 can be provided in the first wafer 10. An angled portion 18 is provided at the outer periphery of the first wafer 10. Figure 2B and Figure 2C As shown, in the bevel portion 18 , the thickness becomes thinner as it is closer to the edge 17 of the first wafer 10 .
[0044] The upper surface 15 of the first wafer 10 is a portion excluding the beveled portion 18. The upper surface 15 is, for example, along the c-plane of sapphire constituting the first wafer 10. For example, the angle between the upper surface 15 and the c-plane of sapphire is less than 5°. It should be noted that the upper surface 15 may also be inclined relative to the c-plane of sapphire.
[0045] In the upper surface 15 of the first wafer 10, a first direction V1 and a second direction V2 are set. The first direction V1 and the second direction V2 are both directions parallel to the upper surface 15. In the present embodiment, six directions are set respectively. As described later, when the semiconductor layer 20 is formed on the upper surface 15 of the first wafer 10, the first direction V1 is a direction passing through the center C of the first wafer 10 and parallel to the m-axis of the semiconductor layer 20. Furthermore, when the semiconductor layer 20 is formed on the upper surface 15 of the first wafer 10, the second direction V2 is a direction passing through the center C and parallel to the a-axis of the semiconductor layer 20. The center C of the first wafer 10 is the center of the circumscribed circle of the first wafer 10 when viewed from above. For example, the angle formed by the first directions V1 is 60°. For example, the angle formed by the second directions V2 is 60°. For example, the angle formed by the adjacent first direction V1 and the second direction V2 is 30°.
[0046] The upper surface 15 of the first wafer 10 includes a first region 11 and a second region 12. The second region 12 is arranged around the first region 11 and is located at a lower position than the first region 11. Therefore, a step portion 16 is formed between the first region 11 and the second region 12. For example, the second region 12 is located at a position lower than the first region 11 by more than 2 μm. In other words, the height G of the step portion 16 is, for example, more than 2 μm, for example, 6 μm. There is no particular upper limit to the height G of the step portion 16. The upper limit of the height G of the step portion 16 is, for example, less than 30 μm.
[0047] In a plan view, the first region 11 has a shape in which six extension portions 14 extend from the outer edge of one circular portion 13 along the first direction V1 toward the end edge 17 of the first wafer 10. For example, the center of the circular portion 13 coincides with the center C of the first wafer 10. The extension length of each extension portion 14 is, for example, not less than 0.1 mm and not more than 10 mm, preferably not less than 0.5 mm and not more than 5 mm.
[0048] Therefore, the first distance D1 between the end edge 17 of the first wafer 10 and the first region 11 in the first direction V1 is shorter than the second distance D2 between the end edge 17 of the first wafer 10 and the first region 11 in the second direction V2 by the extension length of the extension portion 14. That is, the relationship between the first distance D1 and the second distance D2 is first distance D1<second distance D2. The first distance D1 is, for example, greater than 0.1 mm and less than 5 mm, preferably greater than 0.2 mm and less than 3 mm. The second distance D2 is, for example, greater than 1 mm and less than 10 mm.
[0049] The second region 12 is sandwiched between the rounded portion 13 and the beveled portion 18. In contrast, the second region 12 may or may not exist between the extended portion 14 and the beveled portion 18. Figure 2A and Figure 2B In the example shown, the extension portion 14 does not reach the bevel portion 18 , and the second region 12 is present between the extension portion 14 and the bevel portion 18 .
[0050] (Step of Forming Semiconductor Layer 20)
[0051] Then, if Figure 1 As shown in step S2 , a semiconductor layer 20 composed of a nitride semiconductor is formed on the first wafer 10 .
[0052] Figure 3A 1 is a plan view showing the first wafer 10 and the semiconductor layer 20 in this embodiment.
[0053] Figure 3B It is along Figure 3A A partial cross-sectional view in the first direction V1 is shown.
[0054] Figure 3C It is along Figure 3A A partial cross-sectional view in the second direction V2 is shown.
[0055] Figure 4A It is a plan view showing the crystal orientation of the semiconductor layer 20 .
[0056] Figure 4B It is a perspective view showing the crystal orientation of the semiconductor layer 20 forming a hexagonal crystal structure.
[0057] like FIG. 3A to FIG. 3C As shown, for example, the first wafer 10 is used as a substrate for crystal growth, and a semiconductor layer 20 is epitaxially grown on the upper surface 15 of the first wafer 10 by a vapor deposition method such as MOCVD (Metal Organic Chemical Vapor Deposition). The semiconductor layer 20 includes, for example, a III-V group nitride semiconductor (In X AlY Ga 1-X-Y N(0≤X, 0≤Y, X+Y≤1)). The semiconductor layer 20 includes, for example, an n-type semiconductor layer, a p-type semiconductor layer, and a light-emitting layer located between the n-type semiconductor layer and the p-type semiconductor layer. The peak wavelength of light emitted from the light-emitting layer is, for example, greater than 330nm and less than 400nm. When the peak wavelength of light emitted from the light-emitting layer is greater than 330nm and less than 400nm, when the semiconductor layer 20 includes a semiconductor layer that does not contain aluminum (Al), for example, gallium nitride (GaN), the light from the light-emitting layer is easily absorbed by the semiconductor layer. By making the semiconductor layer 20 include a layer containing Al, for example, an AlGaN layer, a high transmittance relative to the light emitted from the light-emitting layer can be obtained. The semiconductor layer 20 includes, for example, Al x1 Ga 1-x1 N(0.03≤x1≤0.08).
[0058] At this time, the film thickness of the peripheral portion of the semiconductor layer 20 becomes thicker than the film thickness of other portions of the semiconductor layer 20. Here, the peripheral portion of the semiconductor layer 20 refers to, for example, a portion of the semiconductor layer 20 located at the end of the first region 11. In the case where the semiconductor layer 20 includes a layer containing Al, the film thickness of the peripheral portion of the semiconductor layer 20 tends to be thicker than other regions of the semiconductor layer 20 more significantly than in the case where the semiconductor layer 20 does not contain Al. It is believed that the reason is that in the case where the semiconductor layer 20 includes a semiconductor layer containing Al, unexpected growth is likely to occur in the peripheral portion of the semiconductor layer 20. In addition, the film thickness of the peripheral portion of the semiconductor layer 20 depends on the direction from the center C, and the film thickness t1 of the end located in the first direction V1 as viewed from the center C is thicker than the film thickness t2 of the end located in the second direction V2 as viewed from the center C. That is, the relationship between the film thickness t1 and the film thickness t2 is film thickness t1>film thickness t2. The semiconductor layer 20 formed on the first region 11 has an end portion located in the first direction V1 as viewed from the center C, i.e., a portion having a thickness of t1 or a value close to t1 as a thick film portion 20a. There are six thick film portions 20a located at the end portion of the semiconductor layer 20 as viewed from the center C in the first direction V1.
[0059] The reason why the film thickness becomes non-uniform in this way is not necessarily clear, but it is estimated as follows, for example. As described above, the first direction V1 is along the m-axis of the semiconductor layer 20, and the second direction V2 is along the a-axis of the semiconductor layer 20. Figure 4A and Figure 4BAs shown, the (0001) c-plane of the semiconductor layer 20 is parallel to the upper surface 15 of the first wafer 10. In this case, the crystal growth rate along the m-axis (first direction V1) of the semiconductor layer 20 relative to the (0001) c-plane of the semiconductor layer 20 is slower than the crystal growth rate along the a-axis (second direction V2) of the semiconductor layer 20. Therefore, it is estimated that the film thickness of the end portion of the semiconductor layer 20 in the first direction V1 where the crystal growth rate relative to the (0001) c-plane of the semiconductor layer 20 is slow is thicker than the surrounding portion because the crystal growth in the second direction V2, which is faster than the first direction V1, also affects the crystal growth in the first direction V1 and promotes the crystal growth.
[0060] In the first region 11 of the first wafer 10, an extension portion 14 is provided in the first direction V1 as viewed from the center C, and the first distance D1 is shorter than the second distance D2. Therefore, the thick film portion 20a of the semiconductor layer 20 is located on the outer peripheral side of the first wafer 10 compared to the end portion of the semiconductor layer 20 in the second direction V2. The thick film portion 20a of the semiconductor layer 20 is formed in the region where the extension portion 14 is provided in the first region 11.
[0061] (Step of Bonding the Second Wafer 30)
[0062] Then, if Figure 1 As shown in step S3, the second wafer 30 is bonded to the first wafer 10 via the semiconductor layer 20. The second wafer 30 is, for example, a silicon wafer.
[0063] Figure 5 FIG. 1 is a bottom view showing the second wafer 30 in this embodiment.
[0064] Fig. 6A 1 is a plan view showing the first wafer 10 , the semiconductor layer 20 , and the second wafer 30 in this embodiment.
[0065] Figure 6B It is along Fig. 6A A partial cross-sectional view in the first direction V1 is shown.
[0066] Figure 6C It is along Fig. 6A A partial cross-sectional view in the second direction V2 is shown.
[0067] like Figure 5 , FIG. 6A to FIG. 6C As shown, the lower surface 31 of the second wafer 30 includes a flat portion 32 and an inclined portion 33. When viewed from above, the shape of the flat portion 32 is substantially circular, for example, the center of the flat portion 32 coincides with the center C of the first wafer 10. The inclined portion 33 is disposed around the flat portion 32. The inclined portion 33 is inclined from the flat portion 32 toward the upper surface 35 of the second wafer 30.
[0068] Similarly, the upper surface 35 of the second wafer 30 includes a flat portion 36 and an inclined portion 37. For example, when viewed from above, the flat portion 36 of the second wafer 30 substantially overlaps with the flat portion 32 of the first wafer 10, and the inclined portion 37 substantially overlaps with the inclined portion 33. The inclined portion 37 is inclined from the flat portion 36 toward the lower surface 31 of the second wafer 30. Therefore, the outer periphery of the second wafer 30 becomes thinner toward the end edge. The width of the inclined portion 33 and the inclined portion 37 is, for example, about 700 μm. The inclined portion 33 and the inclined portion 37 are, for example, beveled portions of the second wafer 30.
[0069] Furthermore, in the process of bonding the second wafer 30 to the first wafer 10, the end of the first wafer 10 located in the first direction V1 as viewed from the center C is made to face and bond with the inclined portion 33 of the second wafer 30. Thus, the thick film portion 20a of the semiconductor layer 20 faces the inclined portion 33 of the second wafer 30. The inclined portion 33 is located above the flat portion 32, so when bonding the semiconductor layer 20 of the first wafer 10 and the second wafer 30, the thick film portion 20a can be avoided from contacting the second wafer 30, and the flat portion 32 of the second wafer 30 can be made to contact with the flat portion of the semiconductor layer 20 other than the thick film portion 20a. As a result, the second wafer 30 can be reliably bonded to the first wafer 10 via the semiconductor layer 20.
[0070] Afterwards, the structure including the first wafer 10, the semiconductor layer 20, and the second wafer 30 is processed using the second wafer 30 as a supporting substrate. For example, the first wafer 10 as a substrate for crystal growth can be peeled off from the semiconductor layer 20. After the first wafer 10 is peeled off, the structure including the semiconductor layer 20 and the second wafer 30 is singulated. In this way, a plurality of semiconductor elements are manufactured from the structure including the second wafer 30 and the semiconductor layer 20. The semiconductor element is a light-emitting element such as a light-emitting diode (LED).
[0071] Next, the effects of this embodiment will be described.
[0072] In the method for manufacturing a semiconductor element of the present embodiment, a first region 11 and a second region 12 are provided on the upper surface 15 of a first wafer 10. Thus, when a semiconductor layer 20 is formed on the upper surface 15, the end of the semiconductor layer 20 is formed in the second region 12. A step portion 16 is formed between the first region 11 and the second region 12, so that the progress of a crack generated in the end of the semiconductor layer 20 is prevented by the step portion 16 and is difficult to enter the portion of the semiconductor layer 20 formed in the first region 11. Thus, the crack density in the semiconductor layer 20 can be reduced, and semiconductor elements can be formed with a good yield.
[0073] Furthermore, according to the present embodiment, an extension portion 14 is provided in a region of the first region 11 that is located in the first direction as viewed from the center C. Thus, a first distance D1 between the edge 17 and the first region 11 in the first direction V1 as viewed from the center C is made shorter than a second distance D2 between the edge 17 and the first region 11 in the second direction V2 as viewed from the center C. As a result, the thick film portion 20a of the semiconductor layer 20 is located at a portion closer to the outer side of the extension portion 14 than the outer edge of the circular portion 13, and is opposite to the inclined portion 33 of the second wafer 30 when the first wafer 10 and the second wafer 30 are bonded. Thus, the thick film portion 20a can be prevented from contacting the second wafer 30. As a result, the second wafer 30 is tightly attached to the semiconductor layer 20 and stably fixed. Thus, the subsequent process of using the second wafer 30 as a supporting substrate becomes stable.
[0074] Therefore, according to the present embodiment, the yield of semiconductor elements can be improved and the process can be performed stably, so that the productivity of semiconductor elements can be improved.
[0075] <Comparative Example>
[0076] Next, comparative examples will be described.
[0077] Fig. 7A It is a top view showing the method for manufacturing the semiconductor element according to this comparative example.
[0078] Figure 7B It is a partial cross-sectional view showing the method for manufacturing the semiconductor element according to this comparative example.
[0079] like Fig. 7A and Figure 7B As shown, in this comparative example, the second region is not provided on the upper surface 115 of the first wafer 110. Therefore, the upper surface 115 is flat as a whole. In addition, a semiconductor layer 120 is formed on the upper surface 115 of the first wafer 110. As described in the above embodiment, the film thickness of the outer peripheral portion of the semiconductor layer 120 is relatively thick. In particular, a thick film portion 120a having a thicker film thickness than the end portions in other directions is formed at the end portion of the semiconductor layer 120 located in the first direction V1 as viewed from the center C.
[0080] Next, the second wafer 30 is bonded to the first wafer 110 via the semiconductor layer 120. At this time, the thick film portion 120a of the semiconductor layer 120 faces the inclined portion 33 of the second wafer 30, so that the thick film portion 120a and the second wafer 30 can be prevented from contacting each other.
[0081] However, when the semiconductor layer 120 is formed using the first wafer 110 whose upper surface 115 is flat as a whole as in the present comparative example, unexpected growth of the semiconductor layer occurs at the end of the semiconductor layer 120, and there is a case where a crack 121 is generated from this portion. Moreover, in the present comparative example, the upper surface 115 of the first wafer 110 is flat, and no step portion is formed anywhere on the upper surface 115, so the crack 121 generated at the end of the semiconductor layer 120 is easy to propagate to the central portion of the semiconductor layer 120. As a result, the yield of the semiconductor layer 120 decreases, and the productivity of the semiconductor element decreases. It should be noted that cracks at the end of the semiconductor layer 120 are easy to occur when the semiconductor layer 120 includes a semiconductor layer containing aluminum (Al). This is presumed to be that when the semiconductor layer 120 includes a semiconductor layer containing Al as described above, unexpected growth of the semiconductor layer is easy to occur at the end of the semiconductor layer 120, and cracks are easy to occur in this portion.
[0082] <Reference example>
[0083] Next, a reference example will be described.
[0084] Fig. 8A It is a top view showing the method for manufacturing the semiconductor element according to this reference example.
[0085] Figure 8B It is a partial cross-sectional view showing the method for manufacturing the semiconductor element according to this reference example.
[0086] like Fig. 8A and Figure 8B As shown, in this reference example, a first region 211 and a second region 212 are provided on the upper surface 215 of the first wafer 210. However, no extension portion is provided in the first region 211, and the outer edge of the first region 211 is circular when viewed from above. Therefore, the thick film portion 220a of the semiconductor layer 220 is formed at a position formed in the first direction V1 as viewed from the center C at the outer periphery of the portion of the semiconductor layer 220 provided in the first region 211. The outer shape of the first wafer 210 is substantially the same as the outer shape of the second wafer 30. In this case, no extension portion is provided in the first region 211, so the thick film portion 220a abuts against the flat portion 32 of the lower surface 31 of the second wafer 30.
[0087] In this reference example, the second region 212 is provided on the upper surface 215 of the first wafer 210, so even if a crack is generated in the end of the semiconductor layer 220, the advancement of the crack is blocked by the step portion 216 between the first region 211 and the second region 212. Therefore, the crack generated in the end of the semiconductor layer 220 is difficult to propagate toward the central portion of the semiconductor layer 220.
[0088] However, in this reference example, when the second wafer 30 is bonded to the first wafer 210 via the semiconductor layer 220, there is a possibility of failure. Specifically, since the thick film portion 220a of the semiconductor layer 220 is in contact with the flat portion 32 of the second wafer 30, the portion of the semiconductor layer 220 other than the thick film portion 220a is not well abutted against the second wafer 30, resulting in a bonding failure. As a result, the structure composed of the first wafer 210, the semiconductor layer 220, and the second wafer 30 becomes unstable in the subsequent process, and the productivity of the semiconductor element decreases.
[0089] <Test example>
[0090] Next, test examples will be described.
[0091] Fig.9A 1 is a plan view showing the first wafer 110 and the semiconductor layer 120 in this experimental example.
[0092] Fig. 9B The horizontal axis represents the radial position and the vertical axis represents the height of the upper surface of the semiconductor layer 120. Fig.9A The graph of the shape of the semiconductor layer 120 along the line segment AA′ is shown.
[0093] Fig. 9C The horizontal axis is the angle θ and the vertical axis is the protrusion H to represent the Fig.9A Circle B is a graph of the shape of semiconductor layer 120 shown.
[0094] It should be noted that the angle θ is an angle observed from the center C of the first wafer 110, and the direction of θ=0° coincides with one of the second directions V2. Furthermore, the protrusion H is the difference between the height of the edge of the semiconductor layer 120 and the height of a position 70 μm away from the edge of the semiconductor layer 120 toward the center C. Fig. 9B and Fig. 9C For example, it is the measurement result of a surface roughness meter.
[0095] In this experimental example, a semiconductor layer 120 including a gallium nitride semiconductor is epitaxially grown on a first wafer 110 made of sapphire by MOCVD. The semiconductor layer 120 includes an n-type semiconductor layer, a p-type semiconductor layer, and a light-emitting layer located between the n-type semiconductor layer and the p-type semiconductor layer. It should be noted that in this experimental example, the aforementioned comparative example, and the reference example, the semiconductor layer is formed under the same conditions. The average thickness of the semiconductor layer 120 is set to 10 μm.
[0096] like Fig. 9B As shown, the end portion of the semiconductor layer 120 is thicker than other portions.
[0097] like Fig. 9CAs shown, the film thickness of the end of the semiconductor layer 120 has angle dependence, and when viewed from the center C, the protrusion H in the portion located in the second direction V2 is about 1.5 to 3 μm, and the protrusion H in the portion located in the first direction V1 is about 4 to 5 μm. That is, the end on the first direction V1 side is thicker than the end on the second direction V2 side.
[0098] Therefore, as in the aforementioned reference example, when the outer shape of the first region 211 is made circular, the thick film portion 220a of the semiconductor layer 220 contacts the flat portion 32 of the second wafer 30, resulting in poor bonding. It should be noted that it is also considered to widen the width of the inclined portion 33 of the second wafer 30 to avoid the thick film portion 220a from contacting the flat portion 32. In addition, it is also considered to make the first wafer 210 larger than the second wafer 30 to avoid the thick film portion 220a from contacting the flat portion 32. However, the size and shape of the wafer are standardized. If they are changed, the specifications of most of the processing equipment used in the manufacture of semiconductor elements need to be changed, resulting in a significant reduction in the productivity of semiconductor elements. In addition, there is a problem of reducing the yield of semiconductor elements that can be manufactured in one manufacturing process.
[0099] In contrast, according to the above-described embodiment, the propagation of cracks can be suppressed and the thick film portion 20 a can be prevented from contacting the second wafer 30 by using wafers of existing specifications, thereby enabling semiconductor devices to be manufactured with good productivity.
[0100] Industrial Applicability
[0101] The present invention can be used in the manufacture of semiconductor elements such as light emitting diodes (LEDs) and laser diodes (LDs).
Claims
1. A method for manufacturing a semiconductor element, characterized in that: have: A step of forming a semiconductor layer composed of a nitride semiconductor by epitaxial growth on a first wafer composed of sapphire; a step of bonding a second wafer to the first wafer via the semiconductor layer; The upper surface of the first wafer includes a first region and a second region, wherein the second region is arranged around the first region and is located at a lower position than the first region. When the first wafer is viewed from above, a first distance between the end edge of the first wafer and the first region in a first direction passing through the center of the first wafer and parallel to the m-axis of the semiconductor layer is shorter than a second distance between the end edge of the first wafer and the first region in a second direction passing through the center of the first wafer and parallel to the a-axis of the semiconductor layer. The lower surface of the second wafer includes a flat portion and an inclined portion, the inclined portion is arranged around the flat portion and is inclined from the flat portion toward the upper surface. In the step of bonding the second wafer, the end portion of the first wafer located in the first direction is bonded to the inclined portion of the second wafer so as to face each other.
2. The method for manufacturing a semiconductor device according to claim 1, wherein: The film thickness of the semiconductor layer in the first region at an end portion located in the first direction is thicker than the film thickness of the semiconductor layer in the first region at an end portion located in the second direction.
3. The method for manufacturing a semiconductor element according to claim 1 or 2, wherein: The second region is located at a position lower than the first region by 2 μm or more.
4. The method for manufacturing a semiconductor element according to claim 1 or 2, wherein: The second distance is greater than or equal to 1 mm and less than or equal to 10 mm.
Citation Information
Patent Citations
Epitaxial growth substrate, semiconductor device, and epitaxial growth method
WO2011161975A1
Nitride semiconductor light-emitting device
JP2011091251A
Heterogeneous annealing method and device
US20140061942A1