Multi-layer metal-clad electric spark cutting wire and manufacturing method thereof
By using a multi-layer cladding structure of ferroalloy inner core, copper layer and brass layer in the electric spark cutting wire, the problems of high cost of electrode wire material, slow cutting speed and poor finish are solved, and high conductivity and mechanical strength are achieved And smooth cutting surfaces, suitable for fine processing.
Patent Information
- Application Number
- CN202010944982.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-09-10
AI Technical Summary
The existing electrode wire materials for electric spark processing are costly, slow cutting speed, poor surface finish, and difficult to process extremely fine parts.
EDM wires coated with multi-layer metal, including ferroalloy inner core, copper layer and brass layer, are formed by coating to form a closely-bonded composite structure, improve conductivity and mechanical strength, and achieve smooth cutting through zinc gasification noodle.
It achieves high conductivity, mechanical strength and smooth cutting surfaces, and can quickly process tiny workpieces, reduce the use of precious metal materials, and improve cutting speed and stability.
Smart Images

Figure CN111906163B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrode wire for metal conductive parts machined by electric spark machining, and in particular to an electrode wire of double-layer and multi-layer composite metal material and a manufacturing method thereof. Background Art
[0002] Electrospark machining is a method of machining workpieces through the electro-erosion effect of pulse discharge between the electrospark cutting electrode wire and the workpiece electrode. At present, wire cutting electrode wires are divided into slow wire and fast wire. Fast wire uses molybdenum wire and tungsten wire to make cutting wires. The conductivity of molybdenum wire is about 30%, and molybdenum wire and tungsten wire have high strength, which can be cut relatively quickly. However, both materials are precious metals. On the one hand, the material cost is high, and on the other hand, it is difficult to draw. Moreover, there is no vaporized metal on the surface of molybdenum wire and tungsten wire, and its cutting surface is relatively rough. Usually, after fast wire processing, it is necessary to use slow wire for surface finishing. Half of the slow wire uses brass wire. The conductivity of brass wire is about 20%, the material strength is low, and the drawing performance is poor. Therefore, the wire diameter of the cutting wire is thicker and easy to break. Due to the high zinc content, it is difficult to draw the diameter of the microwire, so it is impossible to process extremely fine parts. In addition, brass wire has slow cutting speed and is easy to change the wire diameter during use, which affects the use.
[0003] In addition, some copper-clad steel composite wires are used to make electrode wires, but they generally have the disadvantages of low conductivity (generally 15-25%) and poor pulse current stability. Moreover, the copper-clad steel composite materials commonly used in the market are mainly produced by electroplating. The electroplating process requires the use of toxic cyanide, which will cause serious pollution to the environment during the production process. Toxic substances will also remain in the finished product. In addition, the bonding strength of copper and steel is poor and easy to wear. Copper powder is very likely to fall off during the cutting process, affecting the surface finish of the cut workpiece.
[0004] The above information is presented as background information only to assist with an understanding of the present disclosure. No determination has been made, and no assertion is made, as to whether any of the above might be applicable as prior art with respect to the present disclosure. Summary of the invention
[0005] The purpose of the present invention is to solve the problems of poor surface finish and high cost of fast wire cutting wire and slow cutting speed and poor processing of slow wire cutting wire in the prior art. To this end, the present invention proposes a multi-layer metal-clad electric spark cutting wire and a manufacturing method of the cutting wire.
[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a multi-layer metal-coated electric spark cutting wire, comprising an iron alloy inner core capable of providing support for high strength, a copper layer continuously coated on the outer side of the inner core, and a brass layer continuously coated on the outer side of the copper, the copper layer is tightly combined with the inner core to form a copper infiltration layer, the brass and the copper layer form atomic bites, the copper layer has a higher conductivity than the inner core and the brass layer, and the brass layer has a lower melting and gasification temperature than the copper layer and the inner core.
[0007] In the above technical solution, further, the thickness of the copper layer is 0.01-0.1 mm, and the area ratio of the copper layer in the cross section of the multi-layer metal-coated electric spark cutting wire is 15-40%.
[0008] Optionally, the brass layer contains 30%-50% zinc by weight, and the thickness of the brass layer is 0.01-0.1 mm.
[0009] Optionally, the inner core is one of high carbon steel, medium carbon steel, low carbon steel, alloy steel or stainless steel.
[0010] Optionally, the diameter of the multi-layer metal-coated electric spark cutting wire is between 0.01-0.50 mm.
[0011] The present invention also provides a multi-layer metal-clad electric spark cutting wire and a manufacturing method thereof, which comprises the following steps:
[0012] S1. Select the raw steel rod, clean and pre-treat the surface of the steel rod to make its surface clean and free of oil stains;
[0013] S2. Pulling the steel rod to a predetermined wire diameter;
[0014] S3. Configure copper belt;
[0015] S4. The copper strip is continuously deformed longitudinally by a coating machine, and is continuously coated on the outside of the steel rod in the longitudinal direction, and the seams of the copper strip are continuously welded to form a copper-clad steel rod;
[0016] S5, drawing the copper-clad steel rod with a die having a compression amount of 10-30% to obtain a copper-clad steel billet;
[0017] S6. Clean and grind the surface of copper-clad steel blank;
[0018] S7. Configuration brass strip, the brass strip containing 30%-50% by weight of zinc;
[0019] S8, using a cladding machine to continuously deform the brass strip longitudinally, and continuously clad the brass strip longitudinally on the outside of the copper-clad steel blank, and continuously weld both sides of the brass strip to form a double-layer copper-clad steel rod;
[0020] S9, drawing the coated double-layer copper-clad steel rod with a die having a compression amount of 10-30%, so that the copper and the brass form a close combination, and obtaining a double-layer copper-clad steel blank;
[0021] S10, heat treating the double-layer copper-clad steel blank at a temperature of 500-700° C., and then continuously drawing to obtain a multi-layer metal-clad electric spark cutting wire of a specified wire diameter.
[0022] In the above technical scheme, it is further preferred that in step S1, a raw steel rod with a diameter of 7 to 15 mm is selected; in step S4, a copper strip is coated and welded on the outside of the steel rod using a coating machine with a diameter of 10 mm to 14 mm; in step S8, a brass strip is coated on the outside of the copper-clad steel billet using a coating machine with a diameter of 8 mm to 12 mm.
[0023] Optionally, in step S3, a copper strip is provided according to 20%-50% of the volume of the drawn steel rod, and the thickness of the copper strip is 0.2-0.9 mm.
[0024] Optionally, in step S7, a brass strip is configured according to 20%-50% of the volume of the copper-clad steel billet, and the thickness of the brass strip is 0.2-0.9 mm.
[0025] Optionally, in step S10, the heat-treated double-layer copper-clad steel billet is continuously drawn to a wire diameter between 0.01-0.50 mm.
[0026] The present invention adopts a coating method to coat two kinds of copper and brass on the surface of steel in sequence, so that the copper and the steel surface are tightly combined to form an effective physical bonding layer, and atomic bite is formed between the copper and the brass. The three metal compounds have their own characteristics. The steel can provide tensile strength, so that the tensile strength of the double-layer coated wire can reach 2000-2600MPa, so that the electric spark cutting wire is easy to machine, and further can be made into a micro wire with a diameter of about 0.02mm; the copper can improve the conductivity of the electric spark cutting wire and stabilize the conductivity, and the conductivity can reach up to 30-50%; the brass layer on the surface has a lower melting point. During wire cutting, the zinc in the brass is gasified to form an airflow, which takes away the shavings on the surface of the object, so that the cutting surface remains smooth and bright.
[0027] Compared with the prior art, the present invention has good machining performance and tensile strength, the conductivity can reach 30%-50%, it can realize fast wire processing, and at the same time can obtain a smooth and smooth cutting surface. In addition, it can be used for fine processing of tiny workpieces. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Attached Figure 1 is a process flow chart of the present invention;
[0029] Attached Figure 2 It is a schematic structural diagram of the multi-layer metal-clad electric spark cutting wire of the present invention.
[0030] Among them: 1. Steel core; 2. Copper layer; 3. Brass layer. DETAILED DESCRIPTION
[0031] The manufacturing method of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0032] First refer to Figure 2 , which shows a cross-section of a multi-layer metal-coated electric spark cutting wire of the present invention. As can be seen from the figure, the metal wire includes: an iron alloy inner core 1 that can provide supporting strength, a copper layer 2 compounded on the outer side of the inner core, and a brass layer 3 coated on the outer side of the copper layer 2. The copper layer 2, the brass layer 3 and the inner core 1 form a double-layer coated composite metal structure. Among them, the inner core 1 can be made of high carbon steel, medium carbon steel, low carbon steel, alloy steel or stainless steel. The inner core mainly supports and increases the tensile strength of the electric spark cutting wire, improves the mechanical processing performance and wire speed of the electric spark cutting wire, and can also be processed into a micro wire of about 0.02mm to achieve fine processing of tiny workpieces.
[0033] The thickness of the copper layer is 0.01-0.1mm, and the area ratio of the copper layer in the cross section of the electric spark cutting wire is 15-40%. The copper can significantly improve the conductivity of the composite wire, improve the stability of the conductivity of the electric spark cutting wire, and save precious metal materials such as molybdenum wire and tungsten wire. The copper layer 2 is tightly combined with the inner core 1 to form a copper infiltration layer, and the thickness of the copper infiltration layer is about 100-1500nm, so the copper layer 2 can be firmly combined with the inner core 1 and will not peel off during cutting.
[0034] The thickness of the brass layer 3 is 0.01-0.1 mm, and the brass layer 3 contains 30-50% zinc by weight, such as brass of models H62 and H70. The brass layer and the copper layer are tightly combined to form atomic bite. During cutting, the zinc in the brass layer vaporizes and takes away the debris on the cutting surface, so that a smooth and smooth cutting surface can be obtained. At the same time, the brass and the copper layer are tightly combined and are not easy to peel off, and the uneven cutting surface caused by the peeling of the copper layer will not be formed.
[0035] Since the structure and properties of the EDM wire vary according to the heat treatment they undergo during the manufacturing process. The EDM wire of the present invention is heat treated during the processing, and the copper atoms in the copper layer diffuse into the steel to form a copper-infiltrated layer. In the case of mutual diffusion, the content of the diffused metal gradually increases from the inner core of the EDM wire to its surface, that is, it is increasingly rich in copper from the core to the surface, and correspondingly, the content of zinc in the brass from the core to the surface is increasing. Since each phase of the brass has different properties, this gives a series of layers with variable properties along the radius of the EDM wire. So that the concentration distribution is adapted to the properties required at each depth: enriched in zinc at the surface, and enriched in copper deeper downward. Therefore, using the present invention, steel, copper and zinc can be alternately deposited in multiple fine layers, that is, on the order of 0.1-1.5 microns. Then the different phases of the brass obtained after heat treatment appear in multiple fine layers (about 0.1-0.5 or 1.5 microns). Thereby, satisfactory mechanical strength, electrical conductivity, fracture strength and high resistance to galvanic wear are obtained.
[0036] Since the key technical node of metal composite materials lies in the bonding strength of two or more materials, the copper layer must be uniform and the bonding strength between the multiple layers of metal must be strong, the present invention adopts the following steps to prepare the electric spark cutting wire (see Figure 1 ):
[0037] (1) Select a steel rod with a diameter of 7-15 mm, perform surface cleaning treatment on it, and remove stains and oxide layers on the surface of the steel rod. The steel rod can be made of high carbon steel, medium carbon steel, low carbon steel, alloy steel or stainless steel. Among them, high carbon steel, alloy steel, stainless steel and medium carbon steel are heat treated in the early stage to soften the material;
[0038] (2) grinding the steel rod with a belt grinder to replace the traditional pickling;
[0039] (3) High-pressure water washing: using water at a pressure of 15-35 MPa to clean surface impurities;
[0040] (4) Drying to remove moisture from the surface of the wire;
[0041] (5) Drawing to the required wire size;
[0042] (6) Degreasing, removing the wire drawing powder and grease remaining from wire drawing, and grinding the surface;
[0043] (7) High-pressure water washing: flush the surface of the wire with a water pressure of 15-35MPa;
[0044] (8) drying the steel rod online for later use;
[0045] (9) A copper strip is provided at 20% to 50% of the volume of the drawn steel rod. In this embodiment, a copper strip with a thickness of 0.2 mm to 0.9 mm is used;
[0046] (10) Using a 10 mm to 14 mm diameter cladding machine, the copper strip is continuously deformed longitudinally and clad on the outside of the steel rod in the longitudinal direction, and the seams of the copper strip are continuously welded by argon arc welding to form a copper-clad steel rod;
[0047] (11) Using a die to draw the copper-clad steel rod, the compression amount is 10-30%, and a copper-clad steel billet with a diameter of 5-10 mm is obtained;
[0048] (12) The surface of the copper-clad steel blank is cleaned to remove the wire drawing powder and the surface is roughened with a sanding machine;
[0049] (13) A brass strip is provided at 20%-50% of the volume of the copper-clad steel blank, and the zinc content of the brass strip is 30%-50%. In this embodiment, the thickness of the brass strip is 0.2-0.9 mm;
[0050] (14) Using a cladding machine with a diameter of 8 mm to 12 mm, the brass strip is continuously deformed and clad on the surface of the copper-clad steel billet in the longitudinal direction, and the two sides of the brass strip are continuously welded to form a double-layer copper-clad steel rod;
[0051] (15) Drawing the coated double-layer copper-clad steel rod with a die having a compression amount of 10-30% to allow the copper and brass to form atomic interlocking to obtain a double-layer copper-clad steel billet;
[0052] (16) The double-layer copper-clad steel blank is annealed at 500-700°C and then continuously drawn to 0.02 mm to obtain a multi-layer metal-clad electrospark cutting wire.
[0053] Preferably, before the material coating welding, the raw material is firstly roughened with a belt sander, which can facilitate the bonding of the contact surfaces of the two metals during the coating process and make the atomic penetration range larger and deeper. In the above-mentioned multiple steps, such as welding, drawing, heat treatment and other processes, they are always carried out in an inert gas protection environment such as argon and nitrogen.
[0054] After the above steps, an electric spark cutting wire with a wire diameter of 0.02mm is finally obtained. The copper layer accounts for 25% of the area in the cross section of the electric spark cutting wire. The tensile strength of the electric spark cutting wire can reach 2500MPa, and the conductivity can reach 40%. The brass layer contains 30-50% zinc, which can increase the air flow on the cutting surface, make the workpiece surface smoother and flatter after cutting, increase the cutting speed, stabilize the pulse current, and the wire speed can reach 8-10m / s.
[0055] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for manufacturing a multi-layer metal-coated electric spark cutting wire, characterized in that: The method comprises the following steps: S1. selecting a raw steel rod, cleaning and pre-treating the surface of the steel rod to make the surface clean and free of oil stains; S2. Pulling the steel rod to a predetermined wire diameter; S3. Configure copper belt; S4. The copper strip is continuously deformed longitudinally by a coating machine, and is continuously coated on the outside of the steel rod in the longitudinal direction, and the seams of the copper strip are continuously welded to form a copper-clad steel rod; S5, drawing the copper-clad steel rod with a die having a compression amount of 10-30% to obtain a copper-clad steel billet; S6. Clean and grind the surface of copper-clad steel blank; S7. Configuration brass strip, the brass strip containing 30%-50% by weight of zinc; S8, using a cladding machine to continuously deform the brass strip longitudinally, and continuously clad the brass strip longitudinally on the outside of the copper-clad steel blank, and continuously weld both sides of the brass strip to form a double-layer copper-clad steel rod; S9, drawing the coated double-layer copper-clad steel rod with a die having a compression amount of 10-30%, so that the copper and the brass form a close combination, and obtaining a double-layer copper-clad steel blank; S10, annealing the double-layer copper-clad steel blank at a temperature of 500-700° C., and then continuously drawing to obtain a multi-layer metal-clad electric spark cutting wire of a specified wire diameter; The multi-layer metal-clad electric spark cutting wire comprises an iron alloy inner core capable of providing high-strength support, a copper layer continuously coated on the outer side of the inner core, and a brass layer continuously coated on the outer side of the copper. The copper layer is tightly combined with the inner core to form a copper infiltration layer, and the thickness of the copper infiltration layer is 100-1500nm; atomic interlocking is formed between the brass and the copper layer, the conductivity of the copper layer is higher than that of the inner core and the brass layer, and the brass layer has a melting and gasification temperature lower than that of the copper layer and the inner core.
2. The method for manufacturing a multi-layer metal-clad electric spark cutting wire according to claim 1, characterized in that: The thickness of the copper layer is 0.01-0.1 mm, and the area ratio of the copper layer in the cross section of the multi-layer metal-clad electric spark cutting wire is 15-40%.
3. The method for manufacturing a multi-layer metal-clad electric spark cutting wire according to claim 1, characterized in that: The brass layer contains 30%-50% zinc by weight, and the thickness of the brass layer is 0.01-0.1 mm.
4. The method for manufacturing a multi-layer metal-clad electric spark cutting wire according to claim 1, characterized in that: The inner core is one of high carbon steel, medium carbon steel, low carbon steel, alloy steel or stainless steel.
5. The method for manufacturing a multi-layer metal-clad electric spark cutting wire according to claim 1, characterized in that: The diameter of the multi-layer metal-clad electric spark cutting wire is between 0.01 and 0.50 mm.
6. The method for manufacturing a multi-layer metal-clad electric spark cutting wire according to claim 1, characterized in that: In step S1, a raw steel rod with a diameter of 7-15 mm is selected; in step S4, a copper strip is coated and welded on the outside of the steel rod using a coating machine with a diameter of 10 mm-14 mm; in step S8, a brass strip is coated on the outside of the copper-clad steel blank using a coating machine with a diameter of 8 mm-12 mm.
7. The method for manufacturing a multi-layer metal-clad electric spark cutting wire according to claim 6, characterized in that: In step S3, a copper strip is arranged according to 20%-50% of the volume of the drawn steel rod, and the thickness of the copper strip is 0.2-0.9 mm.
8. The method for manufacturing a multi-layer metal-clad electric spark cutting wire according to claim 6, characterized in that: In step S7, a brass strip is arranged according to 20%-50% of the volume of the copper-clad steel blank, and the thickness of the brass strip is 0.2-0.9 mm.