Flexible battery, method for preparing the same, and auxiliary battery comprising the same
By applying active substances on the anode and cathode current collector of the lithium-ion battery and controlling the return rate, combined with the separation membrane stacking, the performance degradation and safety problems of the lithium-ion battery during bending are solved, and flexibility and high energy density are achieved battery design.
Patent Information
- Application Number
- CN201980025864.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-11
- Filing Date
- 2019-06-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-06-11
AI Technical Summary
The existing lithium-ion batteries use the fixed form of metal cans, resulting in limited electronic product design, making it difficult to achieve thinning and flexible. The external materials and electrode assembly are prone to breakage when repeatedly bending, resulting in performance degradation and even possible Causes fire or explosion.
By applying active substances to part or all of the anode and cathode current collectors, the composition is formed and vacuum dried, the return rate is controlled to be less than 3.5%, and the separation membrane is laminated to form a pattern of shrinkage and expansion in the length direction when bending is formed. , prevent cracks and performance of the electrode assembly.
It effectively prevents cracks and performance degradation caused by the return positioning phenomenon during the bending process, improves the flexibility and durability of the lithium-ion battery, and ensures the high energy density and safety of the battery.
Smart Images

Figure CN112005415B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a flexible battery, a preparation method thereof and an auxiliary battery comprising the same. Background Art
[0002] As consumer demand shifts toward digitalization and higher performance of electronic products, market demand is also gradually changing toward thinner, lighter, higher-capacity power supply devices with higher energy density.
[0003] In order to meet such consumer demands, power supply devices such as lithium ion secondary batteries, lithium ion polymer batteries, supercapacitors (electric double layer capacitors), and Faraday pseudocapacitors are being developed with high energy density and large capacity.
[0004] Recently, as the demand for mobile electronic devices such as mobile phones, laptops, and digital cameras continues to increase, in particular, flexible mobile electronic devices using roll-up displays, flexible electronic paper (flexible e-paper), flexible liquid crystal displays (flexible-LCD), flexible organic light-emitting diodes (flexible-OLED), etc. have attracted much attention. Therefore, power supply devices for flexible mobile electronic devices need to have flexible characteristics.
[0005] As one of the power supply devices that can reflect this characteristic, flexible batteries are being developed.
[0006] The flexible battery may be a nickel-cadmium battery, a nickel-metal hydride battery, a nickel-hydrogen battery, a lithium-ion battery, etc., which have flexible properties. In particular, compared with other batteries such as lead-acid batteries, nickel-cadmium batteries, nickel-hydrogen batteries, and nickel-zinc batteries, lithium-ion batteries have a high energy density per unit weight and can be quickly charged, thus having a high utilization rate.
[0007] The above lithium-ion battery uses a liquid electrolyte and is mainly used in a welded metal can as a container. However, since the cylindrical lithium secondary battery using a metal can as a container is fixed in shape, it has the following disadvantages, namely, the design of electronic products is limited and it is difficult to reduce the volume.
[0008] In particular, there is a problem that the mobile electronic devices described above have been developed to be thinner, smaller, and more flexible, and therefore existing lithium-ion batteries using metal cans or batteries having a polygonal structure are difficult to apply to the mobile electronic devices described above.
[0009] Therefore, in order to solve the structural problems as described above, recently, a pouch type battery in which an electrolyte is put into a pouch including two electrodes and a separator and used by sealing is being developed.
[0010] This pouch-type battery is made of a flexible material and has the following advantages: it can be prepared into various shapes and has a higher energy density per unit mass.
[0011] Recently, the existing pouch-type batteries as described above have been applied to products in a flexible form. However, if the pouch-type batteries currently in commercial use or under development are repeatedly bent during use, the following problems will occur, namely, the external materials and electrode assemblies may be damaged due to repeated contraction and expansion, and the performance will drop significantly compared to the initial design value, thus limiting the performance of the battery. Damage or low melting point will cause fire and / or explosion when the cathode and anode come into contact, and it is difficult to achieve ion exchange of the electrolyte inside the battery. Summary of the invention
[0012] Technical issues
[0013] The purpose of the present invention proposed to solve the above-mentioned problems is to provide a method for preparing a flexible battery having the following effect, namely, when forming a pattern, the generation of cracks and / or peeling of the active material is prevented by suppressing the retraction phenomenon, thereby preventing performance degradation caused by capacity reduction, resistance increase and internal short circuit.
[0014] Furthermore, another object of the present invention is to provide a flexible battery and an auxiliary battery including the same having the following effects, namely, by forming a prescribed pattern on the electrode assembly, cracks can be prevented from being generated even when bent, and a decrease in the physical properties required of the battery can be prevented or the decrease in the physical properties required of the battery can be minimized even when bent repeatedly.
[0015] Technical Solution
[0016] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing a flexible battery. The flexible battery provided by the present invention is formed by sealing an electrode assembly and an electrolyte together with an external material. The method for preparing the above-mentioned electrode assembly includes: a step of forming an anode composite material by coating a portion or all of at least one side of an anode current collector with an anode active material to form a composition and drying it; a step of preparing an anode by vacuum drying the above-mentioned anode current collector; a step of forming a cathode composite material by coating a portion or all of at least one side of a cathode current collector with a cathode active material to form a composition and drying it; a step of preparing a cathode by vacuum drying the above-mentioned cathode current collector; and a step of stacking by arranging a separation membrane between the above-mentioned anode and the above-mentioned cathode, the back spring rate of the above-mentioned anode composite material calculated by the following mathematical formula 1 is less than 3.5%, and the back spring rate of the above-mentioned cathode composite material calculated by the following mathematical formula 2 is less than 4.5%,
[0017] Mathematical formula 1:
[0018] Restoration rate (%) = ((thickness of anode composite material layer after vacuum drying (μm) / thickness of anode composite material layer before vacuum drying (μm)) - 1) × 100 (%),
[0019] Mathematical formula 2:
[0020] Restoration rate (%) = ((thickness of cathode composite material layer after vacuum drying (μm) / thickness of cathode composite material layer before vacuum drying (μm)) - 1) × 100 (%).
[0021] According to one embodiment of the present invention, the solid content of the anode active material forming composition may be 60 to 90 weight percent, and the vacuum drying of the anode current collector may be performed at a temperature of 90 to 170° C. for 8 to 16 hours.
[0022] Furthermore, the anode active material forming composition may include 0.5 to 1.5 parts by weight of the first conductive material, 0.1 to 1 parts by weight of the second conductive material, and 1 to 4 parts by weight of polyvinylidene fluoride (PVDF) relative to 100 parts by weight of the anode material.
[0023] Furthermore, the solid content of the cathode active material forming composition may be 30 to 65 weight percent, and the vacuum drying of the cathode current collector may be performed at a temperature of 60 to 140° C. for 8 to 16 hours.
[0024] Furthermore, the cathode active material forming composition may include 0.55 to 1.6 parts by weight of the first conductive material and 2.5 to 9 parts by weight of polyvinylidene fluoride relative to 100 parts by weight of the cathode material.
[0025] Furthermore, the first conductive material may include spherical carbon black, and the second conductive material may include graphite.
[0026] Furthermore, the first conductive material may include spherical carbon black.
[0027] Furthermore, the present invention may further include the step of forming a pattern that corresponds to contraction and expansion in the longitudinal direction when the electrode assembly is bent.
[0028] On the other hand, the flexible battery provided by the present invention includes: an electrode assembly, including an anode, a cathode and a separation membrane, wherein the anode is coated with an anode active material on a portion or all of at least one side of the anode current collector, and the cathode is coated with a cathode active material on a portion or all of at least one side of the cathode current collector, and the separation membrane is arranged between the anode and the cathode; an electrolyte; and an external material for sealing the electrode assembly and the electrolyte together, the moisture content of the cathode active material is less than 200 ppm, and the moisture content of the anode active material is less than 500 ppm.
[0029] According to one embodiment of the present invention, the resistance change rate measured by the following measurement method 1 may be less than 5%.
[0030] Determination method 1
[0031] In a fully charged flexible battery, the resistance was measured by bending the battery in the longitudinal direction (Bending) and then bending in the opposite direction, and then the resistance change rate relative to the resistance before bending was measured.
[0032] Furthermore, the thickness of the anode active material layer may be 40 to 60 μm, and the thickness of the cathode active material layer may be 50 to 75 μm.
[0033] Furthermore, the anode active material may be formed by an anode active material forming composition, wherein the anode active material forming composition includes an anode material, a first conductive material, a second conductive material and polyvinylidene fluoride, and the average particle size of the anode material may be 3 to 20 μm.
[0034] Furthermore, the cathode active material may be formed by a cathode active material forming composition, wherein the cathode active material forming composition includes a cathode material, a first conductive material, and polyvinylidene fluoride. The average particle size of the cathode material may be 8 to 40 μm.
[0035] Furthermore, the electrode assembly may include a pattern for coping with contraction and expansion in the longitudinal direction when bent.
[0036] On the other hand, the auxiliary battery provided by the present invention includes: the above-mentioned flexible battery; and a soft shell for covering the surface of the above-mentioned external material, and the above-mentioned shell includes at least one terminal part for electrically connecting to the charging target device.
[0037] Effects of the Invention
[0038] The flexible battery of the present invention has the following effect: when patterning, cracks and / or peeling of active materials are prevented by suppressing the retraction phenomenon, thereby preventing performance degradation caused by capacity reduction, resistance increase, internal short circuit, etc.
[0039] Furthermore, by forming a predetermined pattern, cracks can be prevented from occurring even when the battery is bent, and degradation of the physical properties required for the battery can be prevented or minimized even when the battery is repeatedly bent.
[0040] The flexible battery of the present invention as described above is applicable not only to wearable devices such as smart watches and watchbands, but also to various electronic devices such as rollable displays that require battery flexibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The present invention is a flowchart showing the process of preparing an electrode assembly to be provided in a flexible battery according to an embodiment of the present invention.
[0042] Figure 2 It is an enlarged view showing a partial structure of a flexible battery according to an embodiment of the present invention.
[0043] Figure 3 FIG. 1 is a schematic overall diagram of a flexible battery according to an embodiment of the present invention.
[0044] Figure 4 This is a schematic overall diagram of a flexible battery according to another embodiment of the present invention, showing a case where the first pattern is formed only on the receiving portion side of the external material.
[0045] Figure 5 This is a simplified diagram showing that a flexible battery according to an embodiment of the present invention is embedded in a housing to be implemented as an auxiliary battery.
[0046] Figure 6a This is a photograph showing an anode active material according to an embodiment of the present invention. Figure 6b This is a photograph showing an anode active material that has cracks due to failure to satisfy one embodiment of the present invention.
[0047] Figure 7a This is a photograph showing a cathode active material according to an embodiment of the present invention. Figure 7b This is a photograph showing a cathode active material having cracks due to failure to satisfy one embodiment of the present invention. DETAILED DESCRIPTION
[0048] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings so that a person skilled in the art can easily implement the present invention. The present invention can be implemented by a variety of different embodiments, and the embodiments described herein do not limit the present invention. In order to clearly illustrate the present invention in the accompanying drawings, parts not related to the description are omitted, and the same or similar structural elements are given the same reference numerals throughout the specification.
[0049] like Figure 1 As shown, a flexible battery according to one embodiment of the present invention includes an electrode assembly, and a method for preparing the electrode assembly includes: a step of preparing an anode and a cathode by processing an active material on a part or all of at least one side of an anode current collector and a cathode current collector to form a composition; and a step of stacking by setting a separation membrane between the anode and the cathode.
[0050] Specifically, the preparation method of the above-mentioned electrode assembly includes: a step of forming an anode composite material by coating a portion or all of at least one side of an anode current collector with an anode active material to form a composition and drying it; a step of preparing an anode having an anode active material by vacuum drying an anode current collector having a portion or all of the anode composite material formed on at least one side; a step of forming a cathode composite material by coating a portion or all of at least one side of a cathode current collector with a cathode active material to form a composition and drying it; a step of preparing a cathode having a cathode active material by vacuum drying a cathode current collector having a portion or all of the cathode composite material formed on at least one side; and a step of stacking by arranging a separation membrane between the above-mentioned anode and the above-mentioned cathode.
[0051] First, the step of forming an anode composite material by coating a part or all of at least one surface of an anode current collector with an anode active material forming composition and drying the coating will be described.
[0052] As long as it is a material that can be commonly used as an anode current collector of a flexible battery in the technical field to which the present invention belongs, there is no limitation on the use of the anode current collector, preferably aluminum (Al) can be used. In addition, the thickness of the anode current collector is 10 to 30 μm, preferably 15 to 25 μm.
[0053] The solid content of the above-mentioned anode active material forming composition can be 60 to 90 weight percent, preferably, the solid content can be 65 to 85 weight percent. When the solid content of the above-mentioned anode active material forming composition is less than 60 weight percent, after the electrode is vacuum dried, a return phenomenon will occur, thereby cracks in the electrode may be generated during the forming process of the flexible battery. When it is greater than 90 weight percent, due to the high viscosity of the composition, it is possible to form an uneven coating on the anode collector, thereby possibly reducing the durability to bending. On the other hand, the above-mentioned anode active material forming composition may include an anode material, a first conductive material, a second conductive material and polyvinylidene fluoride.
[0054] As long as it is an anode material that can be commonly used in the technical field to which the present invention belongs, there is no limitation on the use of the above-mentioned anode material. Preferably, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium nickel cobalt oxide (LiNiCoO 2 ), lithium manganese oxide (LiMnO 2 ), lithium manganese tetraoxide (LiMn 2 O 4 ), vanadium pentoxide (V 2 O 5 ), hexavanadium trioxide (V 6 O 13 )、LiNi 1-xy Co x M y O 2 One of lithium transition metal oxides such as lithium nickel cobalt manganese (NCM, Lithium Nickel Cobalt Manganese) (0≤≤x≤≤1, 0≤≤y≤≤1, 0≤≤x+y≤≤1, M is a metal such as Al, Sr, Mg, La, etc.) or a mixture of more than one of them.
[0055] In addition, the average particle size of the anode material may be 3 to 20 μm, preferably, 5 to 15 μm. When the average particle size of the anode material is less than 3 μm, the aggregation of the anode materials may lead to uneven dispersion of the composition or difficulty in moisture management. When the average particle size is greater than 20 μm, cracks may occur in the electrode during the forming process or bending process of the flexible battery.
[0056] As long as it is a conductive material that can be commonly used in the technical field to which the present invention belongs, there is no limitation on the use of the above-mentioned first conductive material. Preferably, spherical carbon black can be included. Relative to 100 parts by weight of the above-mentioned anode material, 0.5 to 1.5 parts by weight of the above-mentioned first conductive material is included, preferably 0.6 to 1.4 parts by weight. When the above-mentioned first conductive material is less than 0.5 parts by weight relative to 100 parts by weight of the above-mentioned anode material, the resistance of the battery may be increased, and when it is greater than 1.5 parts by weight, the capacity of the battery may be reduced.
[0057] Furthermore, as long as it is a conductive material that can be commonly used in the technical field to which the present invention belongs, there is no limitation on the use of the second conductive material, and preferably, graphite can be included. Relative to 100 parts by weight of the anode material, 0.1 to 1 parts by weight of the second conductive material is included, and preferably, 0.2 to 0.9 parts by weight can be included. When the second conductive material is less than 0.1 parts by weight relative to 100 parts by weight of the anode material, the resistance of the battery may increase, and when it is greater than 1 part by weight, the capacity of the battery may decrease.
[0058] In addition, the polyvinylidene fluoride can perform the function of an adhesive between the active material, the conductive material and the current collector, and contains 1 to 4 parts by weight, preferably 1.5 to 3.5 parts by weight, relative to 100 parts by weight of the anode material. When the polyvinylidene fluoride is less than 1 part by weight relative to 100 parts by weight of the anode material, the composite material may be peeled off due to insufficient adhesion, and when it is greater than 4 parts by weight, the resistance may be increased or the capacity of the battery may be reduced.
[0059] On the other hand, the viscosity of the anode active material forming composition is 7000-17000cps at a temperature of 25°C, and preferably, the viscosity at a temperature of 25°C can be 8000-16000cps. When the viscosity of the anode active material forming composition is less than 7000cps at a temperature of 25°C, it is possible that the composition diffuses outside the coating area due to the fluidity of the composition, and when it is greater than 17000cps, the thickness during coating may become uneven.
[0060] On the other hand, the anode active material forming composition may be applied to the anode current collector by press lamination, vapor deposition or coating, but is not limited thereto.
[0061] Furthermore, the drying of the anode active material forming composition may be performed at a temperature of 120 to 180° C. for 0.3 to 3 minutes, but the present invention is not limited thereto.
[0062] Next, a step of vacuum drying the anode current collector having the anode composite material formed on a part or all of at least one surface to prepare an anode having an anode active material will be described.
[0063] As long as the vacuum drying conditions are generally used for preparing anodes, there is no limitation on the above vacuum drying conditions. Preferably, it can be carried out at a temperature of 90 to 170°C for 8 to 16 hours, and more preferably, it can be carried out at a temperature of 100 to 160°C for 9 to 15 hours. If the vacuum drying temperature is less than 90°C or the vacuum drying time is less than 8 hours, the battery will generate gas or increase resistance and capacity due to excessive moisture. If the vacuum drying temperature is greater than 170°C or the vacuum drying time is greater than 16 hours, cracks and / or peeling of the active material may occur during pattern formation due to retraction.
[0064] On the other hand, Figure 6a As shown, in order to prevent cracks and / or peeling of the anode active material when forming a pattern, the back spring of the above-mentioned anode composite material calculated by the following mathematical formula 1 is less than 3.5%, preferably, it can be less than 2.5%, and more preferably, it can be less than 2.0%.
[0065] Mathematical formula 1
[0066] Restoration rate (%) = ((thickness of anode composite material layer after vacuum drying (μm) / thickness of anode composite material layer before vacuum drying (μm)) - 1) × 100 (%)
[0067] If the return rate calculated by the above mathematical formula 1 is greater than 3.5%, then Figure 6b As shown, when patterning is performed, cracks and / or peeling of the anode active material may occur.
[0068] Next, a step of forming a cathode composite material by coating a portion or the entirety of at least one surface of a cathode current collector with a cathode active material-forming composition and drying the coating will be described.
[0069] As long as it is a material that can be commonly used as a cathode current collector of a flexible battery in the technical field to which the present invention belongs, there is no limitation on the use of the cathode current collector, preferably copper (Cu) can be used. In addition, the thickness of the cathode current collector is 3 to 18 μm, preferably 6 to 15 μm.
[0070] The solid content of the cathode active material composition may be 30 to 65 weight percent, preferably 35 to 60 weight percent. When the solid content of the cathode active material composition is less than 30 weight percent, a return phenomenon may occur after vacuum drying, thereby causing cracks in the electrode during the forming process of the flexible battery. When the solid content is greater than 65 weight percent, due to the high viscosity of the composition, an uneven coating may be formed on the collector, thereby reducing the durability to bending.
[0071] On the other hand, the cathode active material forming composition may include a cathode material, a first conductive material and polyvinylidene fluoride.
[0072] There is no limitation on the cathode material, as long as it is a cathode material commonly used in the field. Preferably, it can be selected from the group consisting of crystalline or amorphous carbon, carbon fiber, carbon composite carbon cathode active material, tin oxide, their lithiated, lithium, lithium alloy and a mixture of one or more thereof. Among them, carbon can be one or more selected from the group consisting of carbon nanotubes, carbon nanowires, carbon nanofibers, artificial graphite, graphite, activated carbon, and graphite.
[0073] In addition, the average particle size of the cathode material may be 8 to 40 μm, preferably, 15 to 30 μm. When the average particle size of the cathode material is less than 8 μm, the aggregation of the anode material may lead to uneven dispersion of the composition or difficulty in moisture management. When the average particle size is greater than 40 μm, cracks may occur in the electrode during the forming process or bending process of the flexible battery.
[0074] As long as it is a conductive material that can be commonly used in the technical field to which the present invention belongs, there is no limitation on the use of the above-mentioned first conductive material. Preferably, spherical carbon black can be included. Relative to 100 parts by weight of the above-mentioned cathode material, 0.55 to 1.6 parts by weight of the above-mentioned first conductive material is included, preferably 0.65 to 1.5 parts by weight. Relative to 100 parts by weight of the above-mentioned cathode material, when the above-mentioned first conductive material is less than 0.55 parts by weight, the resistance of the battery may increase, and when it is greater than 1.6 parts by weight, the capacity of the battery may be reduced.
[0075] In addition, the polyvinylidene fluoride can perform the function of an adhesive between the active material, the conductive material and the current collector, and contains 2.5 to 9 parts by weight, preferably 3.5 to 8 parts by weight, relative to 100 parts by weight of the cathode material. When the polyvinylidene fluoride is less than 2.5 parts by weight relative to 100 parts by weight of the cathode material, the composite material may be peeled off due to insufficient adhesion, and when it is greater than 9 parts by weight, the resistance may be increased or the capacity of the battery may be reduced.
[0076] On the other hand, the viscosity of the cathode active material forming composition is 5000-15000cps at a temperature of 25°C, and preferably, the viscosity at a temperature of 25°C can be 6000-14000cps. At a temperature of 25°C, when the viscosity of the cathode active material forming composition is less than 5000cps, it may diffuse outside the coating area due to the fluidity of the composition, and when it is greater than 15000cps, the thickness during coating may become uneven.
[0077] On the other hand, the cathode active material forming composition may be applied to the cathode current collector by lamination, vapor deposition or coating, but is not limited thereto.
[0078] Furthermore, the cathode active material forming composition may be dried at a temperature of 120 to 180° C. for 0.3 to 3 minutes, but the drying process is not limited thereto.
[0079] Next, a step of vacuum drying the cathode current collector having the cathode composite material formed on a part or all of at least one surface to prepare a cathode having a cathode active material will be described.
[0080] As long as the vacuum drying conditions are generally used for preparing cathodes, there is no limitation on the above vacuum drying conditions. Preferably, the vacuum drying can be carried out at a temperature of 60 to 140°C for 8 to 16 hours, and more preferably, at a temperature of 70 to 130°C for 9 to 15 hours. If the vacuum drying temperature is less than 60°C or the vacuum drying time is less than 8 hours, the battery will generate gas or increase resistance and capacity due to excessive moisture. If the vacuum drying temperature is greater than 140°C or the vacuum drying time is greater than 16 hours, the cathode active material may crack and / or peel off when forming a pattern due to retraction.
[0081] On the other hand, Figure 7a As shown, in order to prevent cracks and / or peeling of the cathode active material when forming a pattern, the recovery rate of the above-mentioned cathode composite material calculated by the following mathematical formula 2 is less than 4.5%, preferably, it can be less than 3.5%, and more preferably, it can be less than 3.0%.
[0082] Mathematical formula 2
[0083] Restoration rate (%) = ((thickness of cathode composite material layer after vacuum drying (μm) / thickness of cathode composite material layer before vacuum drying (μm)) - 1) × 100 (%).
[0084] If the return rate calculated by the above mathematical formula 2 is greater than 4.5%, then Figure 7bAs shown, when patterning is performed, cracks and / or peeling of the cathode active material may occur.
[0085] Next, a step of laminating by providing a separation membrane between the anode and the cathode will be described.
[0086] Since the separation membrane can be disposed between the anode and the cathode and stacked by a method commonly used in the technical field to which the present invention pertains, the present invention is not particularly limited thereto.
[0087] On the other hand, the method for preparing a flexible battery of the present invention may further include the step of forming a pattern for coping with the contraction and expansion in the length direction when the electrode assembly is bent.
[0088] When the flexible battery is bent, such a pattern can prevent the substrate from shrinking or expanding, or minimize the shrinkage or expansion of the substrate itself, by offsetting the length change caused by the change in curvature of the bent portion.
[0089] Thus, even if the electrode assembly is repeatedly bent, the amount of deformation of the substrate itself constituting the electrode assembly that may occur locally at the bent portion can be minimized, thereby preventing the electrode assembly from being locally damaged or deteriorating in performance due to bending.
[0090] On the other hand, Figure 2 As shown, a flexible battery 100 according to an embodiment of the present invention includes: an electrode assembly 110, including an anode 112, a cathode 116 and a separation membrane 114, wherein the anode 112 is coated with an anode active material 112b on a part or all of at least one side of the anode current collector 112a, and the cathode 116 is coated with a cathode active material 116b on a part or all of at least one side of the cathode current collector 116a, and the separation membrane 114 is arranged between the anode 112 and the cathode 116; an electrolyte; and an external material 120 for sealing the electrode assembly 110 and the electrolyte together.
[0091] First, the electrode assembly 110 will be described.
[0092] In the description of the electrode assembly, the same parts as those described above will be omitted.
[0093] like Figure 2 As shown, the electrode assembly 110 is sealed together with the electrolyte in an external material 120 to be described later, and may include an anode 112 , a cathode 116 , and a separation membrane 114 .
[0094] The anode 112 includes an anode current collector 112a and an anode active material 112b, and the cathode 116 includes a cathode current collector 116a and a cathode active material 116b. The anode current collector 112a and the cathode current collector 116a may be in the form of a plate-like sheet having a predetermined area.
[0095] On the other hand, the water content of the anode active material 112b is 500ppm or less, preferably, 450ppm or less, and more preferably, 350ppm or less. When the water content of the anode active material 112b is greater than 500ppm, the excessive water may cause the following problems, that is, the battery will generate gas or increase resistance and capacity decrease.
[0096] Furthermore, the thickness of the anode active material 112b may be 40 to 60 μm, preferably 45 to 55 μm. When the thickness of the anode active material 112b is less than 45 μm, the energy density of the battery may be reduced, and when the thickness is greater than 60 μm, cracks in the electrode may occur during the forming process or bending process of the flexible battery.
[0097] On the other hand, the moisture content of the cathode active material 116b is less than 200ppm, preferably, the moisture content may be less than 150ppm, and more preferably, the moisture content may be less than 100ppm. When the moisture content of the cathode active material 116b is greater than 200ppm, the following problems may be caused due to excessive moisture, that is, the battery will generate gas or increase resistance and capacity decrease.
[0098] Furthermore, the cathode active material 116b may have a layer thickness of 50 to 75 μm, preferably 55 to 70 μm. When the layer thickness of the cathode active material 116b is less than 50 μm, the energy density of the battery may be reduced, and when the layer thickness is greater than 75 μm, cracks in the electrode may occur during the forming process or bending process of the flexible battery.
[0099] And, if Figure 2 , Figure 3 , Figure 4 As shown, a cathode terminal 118a and an anode terminal 118b for electrically connecting the body and an external device may be formed on the anode current collector 112a and the cathode current collector 116a, respectively. The anode terminal 118b and the cathode terminal 118a may extend from the anode current collector 112a and the cathode current collector 116a and protrude on one side of the external material 120, and may also be provided in a manner of being exposed on the surface of the external material 120.
[0100] On the other hand, the anode active material 112b and the cathode active material 116b of the present invention may include polytetrafluoroethylene (PTFE) components, which can be used to prevent the anode active material 112b and the cathode active material 116b from peeling off or cracking from the current collectors 112a and 116a, respectively, when bent.
[0101] The anode active material 112 b and the cathode active material 116 b may each contain 0.5 to 20 weight percent of the polytetrafluoroethylene component relative to the total weight. Preferably, the polytetrafluoroethylene may be contained at 5 weight percent or less.
[0102] On the other hand, the separation membrane 114 disposed between the anode 112 and the cathode 116 may include a nanofiber web layer 114 b on one or both sides of the non-woven fabric layer 114 a .
[0103] The nanofiber web layer 114 b may include at least one nanofiber selected from polyacrylonitrile nanofibers and polyvinylidene fluoride nanofibers.
[0104] Preferably, in order to ensure spinnability and form uniform pores, the nanofiber web layer 114b may be composed only of polyacrylonitrile nanofibers, wherein the average diameter of the polyacrylonitrile nanofibers may be 0.1-2 μm, preferably 0.1-1.0 μm.
[0105] This is because when the average diameter of the polyacrylonitrile nanofibers is less than 0.1 μm, the separation membrane may not have sufficient heat resistance, and when it is greater than 2 μm, although the mechanical strength of the separation membrane is excellent, the elasticity of the separation membrane is reduced.
[0106] Furthermore, when a gel polymer electrolyte is used as the electrolyte, the separation membrane 114 may use a composite porous separation membrane to optimize the impregnation property of the gel polymer electrolyte.
[0107] That is, the composite porous separation membrane may be used as a support (matrix) and may include a porous nonwoven fabric having fine pores and a porous nanofiber web impregnated with an electrolyte by being formed of a spinnable polymer material.
[0108] The porous nonwoven fabric may be selected from a polypropylene (PP) nonwoven fabric, a polyethylene (PE) nonwoven fabric, a nonwoven fabric composed of a double structure of polypropylene / polyethylene fibers with a polypropylene fiber as a core and polyethylene coated on the periphery, a nonwoven fabric composed of a polypropylene / polyethylene / polypropylene three-layer structure and having a circuit-breaking function through polyethylene with a relatively low melting point, a polyethylene terephthalate (PET) nonwoven fabric composed of polyethylene terephthalate (PET) fibers, or a nonwoven fabric composed of cellulose fibers. Moreover, the melting point of the polyethylene nonwoven fabric may be 100°C to 120°C, the melting point of the polypropylene nonwoven fabric may be 130°C to 150°C, and the melting point of the polyethylene terephthalate nonwoven fabric may be 230°C to 250°C.
[0109] In this case, preferably, the thickness of the porous nonwoven fabric is set to 10 to 40 μm, the porosity is set to 5 to 55%, and the Gurley value is set to 1 to 1000 sec / 100 c.
[0110] On the other hand, the porous nanofiber web may be made of a swellable polymer that swells in an electrolyte solution alone, or a mixed polymer of a swellable polymer and a heat-resistant polymer that can enhance heat resistance.
[0111] The porous nanofiber web as described above is formed by the following method, that is, after dissolving a single or mixed polymer in a solvent to form a spinning solution, the spinning solution is spun using an electrospinning device, and the spun nanofibers are gathered in a collector to form a porous nanofiber web having a three-dimensional pore structure.
[0112] Among them, for the above-mentioned porous nanofiber web, any polymer can be used as long as it can be spun by an electrospinning method after being dissolved in a solvent to form a spinning solution to form nanofibers. As an example, the above-mentioned polymer can be a single polymer or a mixed polymer, and a swellable polymer, a non-swellable polymer, a heat-resistant polymer, a mixed polymer of a mixed swellable polymer and a non-swellable polymer, a mixed polymer of a mixed swellable polymer and a heat-resistant polymer, etc. can be used.
[0113] In this case, when the porous nanofiber web uses a mixed polymer of a swellable polymer and a non-swellable polymer (or a heat-resistant polymer), the weight ratio of the swellable polymer to the non-swellable polymer is 9:1 to 1:9, and preferably, can be mixed in a weight ratio in the range of 8:2 to 5:5.
[0114] Generally, non-swelling polymers are mostly heat-resistant polymers, and compared with swelling polymers, due to their larger molecular weight, their melting points are relatively higher. Therefore, preferably, the non-swelling polymer is a heat-resistant polymer with a melting point of more than 180°C, and preferably, the swelling polymer is a resin with a melting point of less than 150°C, preferably, it can be a resin with a melting point in the range of 100-150°C.
[0115] On the other hand, the swellable polymer that can be used in the present invention may be a resin that swells in an electrolyte and can be formed into ultrafine nanofibers by an electrospinning method.
[0116] As an example, the swellable polymer may be polyvinylidene fluoride, poly(vinylidene fluoride-co-hexafluoropropylene), a perfluoropolymer, polyvinyl chloride or polyvinylidene chloride and copolymers thereof, polyethylene glycol derivatives including polyethylene glycol dialkyl ethers and polyethylene glycol dialkyl esters, poly(formaldehyde-oligoethylene oxide), polyoxides including polyethylene oxide and polypropylene oxide, polyvinyl acetate, poly(vinyl pyrrolidone-vinyl acetate), polystyrene and polystyrene acrylonitrile copolymers, polyacrylonitrile copolymers including polyacrylonitrile methyl methacrylate copolymers, polymethyl methacrylate, polymethyl methacrylate copolymers, and a mixture of more than one of these.
[0117] Furthermore, as the heat-resistant polymer or non-swelling polymer, a resin having the following characteristics can be used, namely, it can be dissolved in an organic solvent for electrospinning, its swelling rate can be slower than that of a swellable polymer or it can not swell due to the organic solvent contained in the organic electrolyte, and its melting point is above 180°C.
[0118] As an example, the heat-resistant polymer or non-swelling polymer may use polyacrylonitrile (PAN), polyamide fiber, polyimide, polyamide-imide, poly(m-phenylene isophthalamide), polysulfone, polyether ketone, aromatic polyesters such as polyethylene terephthalate, polytrimethylene terephthalate and polyethylene naphthalate, polyphosphazenes such as polytetrafluoroethylene, polydiphenoxy phosphor and poly{bisphosphazene), polyurethane copolymers including polyurethane and polyether carbamate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, etc.
[0119] On the other hand, as the non-woven fabric constituting the above-mentioned non-woven fabric layer 114a, one or more selected from cellulose, cellulose acetate, polyvinyl alcohol (PVA), polysulfone, polyimide, polyetherimide, polyamide, polyethylene oxide (PEO), polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyurethane (PU), polymethyl methacrylate (PMMA) and polyacrylonitrile can be used.
[0120] The nonwoven fabric layer may further include an inorganic additive, and the inorganic additive may include a material selected from SiO, SnO, SnO 2 , PbO 2 、ZnO、P 2 O 5 ,CuO,MoO,V 2 O 5 , B 2 O 3 、Si 3 N 4 、CeO 2 , Mn 3 O 4 Sn 2 P 2 O 7 Sn 2 B 2 O 5 Sn 2 BPO 6 、TiO 2 、BaTiO 3 , Li 2 O, LiF, LiOH, Li 3 N, BaO, Na 2 O. Li 2 CO 3 、CaCO 3 、LiAlO 2 、SiO 2 、Al 2 O 3 and one or more of PTFE.
[0121] Furthermore, the average particle size of the inorganic particles as the inorganic additive may be 10 to 50 nm, preferably 10 to 30 nm, and more preferably 10 to 20 nm.
[0122] Furthermore, the average thickness of the separation membrane may be 10 to 100 μm, preferably 10 to 50 μm. This is because when the average thickness of the separation membrane is less than 10 μm, the long-term durability of the separation membrane cannot be ensured when the battery is repeatedly bent and / or unfolded due to the separation membrane being too thin, and when it is greater than 100 μm, it is not conducive to the thinning of the flexible battery. Therefore, preferably, the separation membrane has an average thickness within the above range.
[0123] Moreover, the average thickness of the nonwoven fabric layer is 10 to 30 μm, preferably 15 to 30 μm. Preferably, the average thickness of the nanofiber web layer is 1 to 5 μm.
[0124] The external material 120 is formed of a plate-shaped member having a predetermined area, and contains the electrode assembly 110 and the electrolyte therein, thereby protecting the electrode assembly 110 from external forces.
[0125] For this reason, Figure 3 and Figure 4 As shown, the external material 120 is composed of a pair of first external material 121 and second external material 122, and is sealed along the edge by an adhesive, thereby preventing the electrolyte and electrode assembly 110 contained therein from being exposed to the outside and leaking to the outside.
[0126] That is, the first external material 121 and the second external material 122 include: a first region S1 having a receiving portion for receiving the electrode assembly and the electrolyte; and a second region S2 arranged to surround the first region S1 and having a sealing portion for preventing the electrolyte from leaking to the outside.
[0127] This external material 120 can be formed by two parts such as the first external material 121 and the second external material 122, and then all edge sides of the sealing part can be sealed by an adhesive, or it can be formed by one part and folded in half along the width direction or the length direction, and then the remaining contact parts can be sealed by an adhesive.
[0128] Furthermore, the external material 120 may include a pattern 124 for responding to the contraction and expansion in the length direction when bent, such as Figure 3 As shown, patterns can be formed in both the first region S1 and the second region S2. Figure 4 As shown, preferably, the pattern 124 may be formed only in the first region S1.
[0129] On the other hand, regarding the content of the pattern of the present invention, reference can be made to Korean Patent No. 10-1680592 of the present inventor, but the detailed description thereof is omitted.
[0130] Furthermore, when the external material 120 does not include a pattern, the external material 120 may use a polymer film with excellent waterproof properties. In this case, due to the flexibility of the polymer film, no additional pattern is required.
[0131] The external material 120 may be formed in a form in which the metal layers 121b and 122b are disposed between the first resin layers 121a and 122a and the second resin layers 121c and 122c. That is, the external material 120 may be formed in a form in which the first resin layers 121a and 122a, the metal layers 121b and 122b, and the second resin layers 121c and 122c are stacked in sequence, the first resin layers 121a and 122a are disposed inside and in contact with the electrolyte, and the second resin layers 121c and 122c are exposed to the outside.
[0132] In this case, the first resin layers 121 a and 122 a seal the external materials 121 and 122 to each other, thereby functioning as a bonding member capable of sealing the electrolyte contained in the battery so as to prevent it from leaking to the outside. The first resin layers 121a and 122a may be made of a material commonly used for joining components of external materials for batteries, and may preferably include a single layer structure or a laminated structure of one of acid-modified polypropylene (PPa), cast polypropylene (CPP), linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), high-density polyethylene (HDPE), polyethylene, polyethylene terephthalate, polypropylene, ethylene vinyl acetate (EVA), epoxy resin and phenolic resin. Preferably, the first resin layers 121a and 122a may be made of a material commonly used for joining components of external materials for batteries, and may preferably include a single layer structure or a laminated structure of one of acid-modified polypropylene (PPa), cast polypropylene (CPP), linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), high-density polyethylene (HDPE), polyethylene, polyethylene terephthalate, polypropylene, ethylene vinyl acetate (EVA), epoxy resin and phenolic resin. It may be composed of a single layer of one kind of Polyethylene) or a stack of two or more kinds thereof.
[0133] Furthermore, the average thickness of the first resin layers 121 a and 122 a may be 20 to 100 μm, and preferably, the average thickness may be 20 to 80 μm.
[0134] This is because, when the average thickness of the above-mentioned first resin layers 121a and 122a is less than 20μm, in the process of sealing the edge sides of the first external material 121 and the second external material 122, it is possible that the bonding force between the contacting first resin layers 121a and 122a will be reduced, and it is not conducive to ensuring the airtightness for preventing electrolyte leakage. When the average thickness is greater than 100μm, it is not only economical but also not conducive to thinning.
[0135] The metal layers 121b and 122b are disposed between the first resin layers 121a and 122a and the second resin layers 121c and 122c to prevent moisture from penetrating from the outside to the housing part and to prevent the electrolyte from leaking from the housing part to the outside.
[0136] To this end, the metal layers 121b and 122b may be formed of dense metal layers to block moisture and electrolyte. The metal layer may be formed by a metal vapor deposition film, that is, the metal vapor deposition film is formed by a known method on a foil-like metal sheet or the second resin layer 121c and 122c described later, such as sputtering, chemical vapor deposition, etc. Preferably, the metal layer may be formed by a metal sheet. When a pattern is formed in this way, cracks in the metal layer may be prevented, thereby preventing the electrolyte from leaking to the outside and preventing moisture from penetrating from the outside.
[0137] As an example, the metal layers 121b and 122b may include one or more selected from aluminum, copper, phosphor bronze (PB), aluminum bronze, nickel silver, beryllium-copper, chromium copper, titanium copper, iron copper, Corson copper-nickel-silicon alloy and chromium-zirconium-copper alloy.
[0138] In this case, the linear expansion coefficient of the metal layers 121b and 122b may be 1.0×10 -7 ~1.7×10 -7 / ℃, preferably, it can be 1.2×10 -7 ~1.5×10 -7 / ℃. This is because when the linear expansion coefficient is less than 1.0×10 -7 / ℃, sufficient flexibility cannot be ensured, so cracks may occur due to external forces generated during bending. When the linear expansion coefficient is greater than 1.7×10 -7 / ℃, there is a possibility of severe morphological deformation due to decreased rigidity.
[0139] The average thickness of the metal layers 121 b and 122 b may be greater than 5 μm, preferably 5 to 100 μm, and more preferably 30 to 50 μm.
[0140] This is because, when the average thickness of the metal layer is less than 5 μm, moisture may penetrate into the interior of the housing portion or the electrolyte in the housing portion may leak to the outside.
[0141] The second resin layers 121c and 122c are located on the exposed surface of the external material 120 to enhance the strength of the external material and prevent damage such as cracks from occurring in the external material due to physical contact applied from the outside.
[0142] The second resin layers 121c and 122c may include at least one selected from nylon, polyethyleneterephthalate (PET), cycloolefin polymer (COP), polyimide (PI) and fluorine compounds, and preferably, may include nylon or fluorine compounds.
[0143] Among them, the above-mentioned fluorine compound may include one or more selected from polytetrafluoroethylene (PTFE), perfluorinated acid (PFA), fluorinatedethelene propylene copolymer (FEP), polytetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), ethylene chlorotrifluoroethylene (ECTFE) and polychlorotrifluoroethylene (PCTFE).
[0144] In this case, the average thickness of the second resin layers 121c and 122c may be 10 to 50 μm, preferably 15 to 40 μm, and more preferably 15 to 35 μm.
[0145] This is because when the average thickness of the second resin layers 121c and 122c is less than 10 μm, the mechanical properties cannot be ensured, and when it is greater than 50 μm, although it is beneficial for ensuring the mechanical properties, it is poor in economic efficiency and is not conducive to thinning.
[0146] On the other hand, the flexible battery 100, 100' of the present invention may further include an adhesive layer between the metal layer 121b, 122b and the first resin layer 121a, 122a.
[0147] The above-mentioned adhesive layer plays a role in improving the bonding force between the metal layer 121b, 122b and the first resin layer 121a, 122a, and at the same time blocks the electrolyte contained in the external material from entering the metal layer 121b, 122b of the external material, thereby preventing the metal layer 121b, 122b from being corroded by the acidic electrolyte and / or the first resin layer 121a, 122a from peeling off from the metal layer 121b, 122b. In addition, even if the flexible battery 100, 100' generates abnormal overheating during use, causing the flexible battery to expand, the electrolyte leakage can be prevented, thereby providing reliability in terms of safety.
[0148] The above-mentioned bonding layer as described above can be formed of a material similar to the first resin layers 121a and 122a so as to improve the bonding force by compatibility with the first resin layers 121a and 122a. As an example, the above-mentioned bonding layer can include one or more selected from silicon, polyphthalate, acid modified polypropylene (PPa) and acid modified polyethylene (Pea).
[0149] In this case, the average thickness of the adhesive layer may be 5 μm to 30 μm, preferably 10 μm to 20 μm, because when the average thickness of the adhesive layer is less than 5 μm, it is difficult to ensure stable bonding force, and when it is greater than 30 μm, it is not conducive to thinning.
[0150] Furthermore, the flexible battery 100, 100' of the present invention may further include a dry laminate layer between the metal layer 121b, 122b and the second resin layer 121c, 122c.
[0151] The dry lamination layer serves to bond the metal layers 121b, 122b and the second resin layers 121c, 122c, and can be formed by using a known aqueous and / or oily organic solvent adhesive.
[0152] In this case, the average thickness of the dry laminate layer may be 1 μm to 7 μm, preferably 2 μm to 5 μm, and more preferably 2.5 μm to 3.5 μm.
[0153] This is because, when the average thickness of the above-mentioned dry laminate layer is less than 1 μm, the poor bonding force may cause peeling between the metal layers 121b, 122b and the second resin layers 121c, 122c. When it is greater than 7 μm, the excessive thickness of the dry laminate layer may have an adverse effect on the formation of a pattern that can cope with shrinkage and expansion.
[0154] On the other hand, the electrolyte sealed in the housing portion together with the electrode assembly 110 may be a generally used liquid electrolyte.
[0155] As an example, an organic electrolyte containing a non-aqueous organic solvent and a lithium salt solute can be used as the above-mentioned electrolyte. Wherein, as the above-mentioned non-aqueous organic solvent, carbonate, ester, ether or ketone can be used. As the above-mentioned carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used, as the above-mentioned ester, butyrolactone (BL), decanolide, valerolactone, mevalonolactone, caprolactone, n-methyl acetate, n-ethyl acetate, n-propyl acetate, etc. can be used, as the above-mentioned ether, butyl ether, etc. can be used, as the above-mentioned ketone, polymethyl vinyl ketone can be used, but the present invention is not limited to the type of non-aqueous organic solvent.
[0156] Furthermore, the electrolyte used in the present invention may contain a lithium salt, which serves as a lithium ion supply source in the battery to achieve the basic operation of the lithium battery. For example, the electrolyte may contain a lithium salt selected from LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiClO 4 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 、LiN(C 2 F 5 SO 2 ) 2 、LiAlO 4 、LiAlCl 4 、LiN(C x F 2x+1 SO 2 )(C y F 2x+1 SO2 )(where x and y are rational numbers) and LiSO 3 CF 3 One or more of the group consisting of or a mixture thereof.
[0157] In this case, although the electrolyte used in the flexible battery 100, 100' of the present invention is generally a liquid electrolyte, preferably, a gel polymer electrolyte may be used, thereby preventing gas leakage and liquid leakage when bending may occur in the flexible battery including the liquid electrolyte.
[0158] The gel polymer electrolyte can be formed by subjecting an organic electrolyte solution containing a non-aqueous organic solvent, a lithium salt solute, a monomer for forming a gel polymer, and a polymerization initiator to a gelation heat treatment to form the gel polymer electrolyte. Although such a gel polymer electrolyte can be formed by subjecting the organic electrolyte to a heat treatment alone, it can be embodied in the following form, that is, by subjecting the separation membrane disposed inside the flexible battery to a heat treatment while being immersed in the organic electrolyte solution to achieve in-situ polymerization of the monomer, so that the gel polymer in a gel state is impregnated in the pores of the separation membrane 114. The in-situ polymerization reaction in the flexible battery can be performed by thermal polymerization, and the polymerization time takes about 20 minutes to 12 hours. The thermal polymerization can be performed at a temperature of 40° C. to 90° C.
[0159] In this case, the above-mentioned monomer for forming a gel polymer is polymerized by a polymerization initiator, and there is no limitation on the use of the polymer as long as it is a monomer that forms a gel polymer, for example, methyl methacrylate (MMA), polyethylene oxide (PEO), polypropylene oxide (PPO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polymethacrylate (PMA), polymethyl methacrylate (PMMA) or a monomer of a polymer thereof, polyacrylate having two or more functional groups such as polyethylene glycol dimethacrylate and polyethylene glycol acrylate.
[0160] In addition, examples of the above-mentioned polymerization initiator include organic peroxide compounds or hydroperoxide compounds such as benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tertbutylperoxide, cumyl hydroperoxide, hydrogen peroxide, etc., and azo compounds such as 2,2-azo(2-cyanobutane) and 2,2-azo(methylbutyronitrile). The above-mentioned polymerization initiator forms a radical by thermal decomposition, and reacts with the monomer by free radical polymerization to form a gel polymer electrolyte, that is, a gel polymer.
[0161] Preferably, the gel polymer forming monomer is used in an amount of 1 to 10 weight percent relative to the organic electrolyte. When the content of the monomer is less than 1 weight percent, it is difficult to form a gel-type electrolyte, and when it is greater than 10 weight percent, the service life is shortened.
[0162] Furthermore, the polymerization initiator may be contained in an amount of 0.01 to 5 weight percent relative to the gel polymer-forming monomer.
[0163] On the other hand, the resistance variation rate of the flexible battery of one embodiment of the present invention measured by the following measurement method 1 may be 5% or less, preferably 3% or less, and more preferably 1% or less.
[0164] Determination method 1
[0165] Under the environmental conditions of temperature of 25°C and humidity of 65%, a hydraulic ram was used to apply 0.8 kN / 24 cm to the fully charged flexible battery along the length of the battery. 2 A load of (=26mm×91.5mm) is applied, thereby causing bending in the range of R25 to R38, and under the same conditions, a load is applied in the opposite direction, thereby causing bending in the range of R25 to R38, and then the resistance is measured for 120 seconds. After the measurement, the resistance is measured at 120 seconds, and thereafter, the resistance change rate relative to the resistance before bending is measured.
[0166] On the other hand, Figure 5As shown, the flexible battery 100 of one embodiment of the present invention includes a housing 130 for covering the surface of the external material 120. The housing 130 may be in the form of an auxiliary battery by including at least one terminal 132 for electrically connecting to a charging target device. Although the housing 130 may be made of a rigid material such as plastic or metal, a flexible soft material such as silicon or leather may also be used.
[0167] Among them, the above-mentioned auxiliary battery can be embodied in accessories such as bracelets, anklets, watch straps, etc., and can be used as fashion items when the above-mentioned charging target device does not need to be charged. When the above-mentioned charging target device needs to be charged, it can be electrically connected to the charging target device through the above-mentioned terminal part 132, so that the main battery of the charging target device can be charged without being restricted by the location.
[0168] Among them, although the figure shows that the terminal parts 132 are arranged in pairs at the ends of the housing 130, it is not limited to this. The terminal parts 131 can be located at the side of the housing 130, or can be formed at various positions such as the upper surface or the lower surface of the housing. In addition, the terminal parts 132 can be formed in a form where the cathode terminal and the anode terminal are separated, or can be formed in a form where the anode and the cathode are combined, such as USB.
[0169] Furthermore, the flexible battery of the present invention can be used as a main battery or auxiliary battery for electrical and / or electronic devices that require flexibility. For example, the flexible battery of the present invention can be widely used in electronic devices such as smart watch straps and flexible displays.
[0170] On the other hand, any preparation method that is commonly used in the technical field to which the present invention pertains to sealing the electrode assembly 110 and the electrolyte together with the external material 120 can be used for the flexible battery 100 of the present invention.
[0171] In this case, the electrode assembly 110 includes: an anode 112, including an anode collector 112a with an anode active material 112b coated on a portion or all of at least one side; and a cathode 116, including a foil-type cathode collector 116a with a cathode active material 116b coated on a portion or all of at least one side, and the electrode assembly 110 includes a pattern to cope with contraction and expansion in the length direction when bent.
[0172] On the other hand, the flexible battery of the present invention has the following effect, that is, in order to improve the flexibility, even if a high-strength pattern is formed, cracks will not be generated in the collector and / or active material. Moreover, as the prescribed pattern is formed, cracks can be prevented from being generated even if bending occurs, and even if bending is repeated, the phenomenon of a decrease in the physical properties required for the battery can be prevented or the decrease in the physical properties required for the battery can be minimized. The flexible battery of the present invention as described above can be applied not only to wearable devices such as smart watches and watchbands, but also to various electronic devices such as rollable displays that require battery flexibility.
[0173] Embodiments of the present invention
[0174] The present invention will be further described in detail below through the following examples, but the following examples do not limit the scope of the present invention and should be interpreted as helping to understand the present invention.
[0175] Example
[0176] First, a metal layer of aluminum material with a thickness of 30 μm is prepared, a first resin layer with a thickness of 40 μm composed of cast polypropylene (CPP) is formed on one side of the metal layer, and a second resin layer with a thickness of 10 μm composed of a nylon film is formed on the other side of the metal layer. In this case, an external material with a total thickness of 85 μm is prepared by arranging a 5 μm acid-modified polypropylene layer in which the content of acrylic acid in the copolymer reaches 6 weight percent between the first resin layer and the metal layer.
[0177] Next, in order to prepare the electrode assembly, first, an anode and a cathode are prepared. The anode is prepared by the following method: an anode current collector made of aluminum with a thickness of 20 μm is coated with an anode active material composition on both sides of the anode current collector at a thickness of 50 μm, and 100 parts by weight of lithium nickel cobalt manganese (NCM) with an average particle size of 10 μm as the anode material is coated with an anode active material composition. Manganese), the anode active material forming composition comprises 1.04 parts by weight of spherical carbon black (Super-P, Timcal) as a first conductive material, 0.52 parts by weight of graphite (KS-6, Timcal) as a second conductive material and 2.6 parts by weight of polyvinylidene fluoride (PVDF), and the anode active material forming composition has a solid content of 75 weight percent and a viscosity of 12000 cps, and then dried at 150°C for 1 minute to form an anode composite material, and then the anode collector with the anode composite material provided on both sides is vacuum dried at 130°C for 12 hours to prepare the anode. Furthermore, the cathode is prepared by the following method, i.e., a cathode active material forming composition is coated on both sides of a cathode collector made of copper with a thickness of 15 μm at a thickness of 60 μm, and the cathode active material forming composition comprises 1.07 parts by weight of spherical carbon black (Super-P, Timcal) as a first conductive material and 5.9 parts by weight of polyvinylidene fluoride (PVDF) relative to 100 parts by weight of artificial graphite with an average particle size of 23 μm as a cathode material, and the solid content of the cathode active material forming composition is 48 weight percent and the viscosity is 10,000 cps, and then the cathode composite material is formed by drying at a temperature of 150°C for 1 minute, and then the cathode collector with the cathode composite material provided on both sides is vacuum dried at a temperature of 100°C for 12 hours to prepare the cathode. Subsequently, a separation membrane made of polyethylene terephthalate / polyethylene naphthalate (PET / PEN) with a thickness of 20 μm was prepared, and an electrode assembly including three anode assemblies, eight separation membranes, and four cathode assemblies was prepared by alternately stacking anode assemblies, separation membranes, and cathode assemblies.
[0178] Subsequently, after folding the prepared external material in such a manner that the first resin layer becomes the inner side, the electrode assembly is arranged inside the external material in such a manner that the first resin layer of the folded external material contacts the electrode assembly, and heat-compression bonding is performed at a temperature of 150°C for 10 seconds in such a manner that only a portion into which the electrolyte can be injected is left. Thereafter, a conventional electrolyte for lithium-ion secondary batteries is injected into the above-mentioned portion, and the portion into which the electrolyte is injected is heat-compressed at a temperature of 150°C for 10 seconds, thereby preparing a battery. Subsequently, by forming the Figure 4 A flexible battery was prepared using the water ripple pattern shown.
[0179] The specific specifications of the prepared flexible battery are shown in Table 1.
[0180] Table 1
[0181] Section thickness (mm) 2.1±0.5 Width(mm) 26.0±0.2 Length (mm, excluding external protruding terminals) 82.0±0.5 Weight(g) 5.2±0.5 Rated capacity (nominal capacity, mAh) 135 Rated voltage (nominal Voltage, V) 3.7
[0182] Example 2 to Example 11 and Comparative Examples 1 to Comparative Examples 7
[0183] A flexible battery was prepared in the same manner as in Example 1 above, except that the vacuum drying conditions of the anode current collector, the vacuum drying conditions of the cathode current collector, the solid content of the anode active material forming composition, and the solid content of the cathode active material forming composition were changed as shown in Tables 3 to 5.
[0184] Experimental Example 1
[0185] 1. Return evaluation
[0186] For the flexible battery prepared by the embodiment and the comparative example, the layer thickness of the anode composite material before vacuum drying and the layer thickness of the cathode composite material before vacuum drying were measured, and the layer thickness of the anode composite material after vacuum drying and the layer thickness of the cathode composite material after vacuum drying were measured, and then the recovery rate was calculated by the following mathematical formula 1 and mathematical formula 2. All of them are shown in Tables 3 to 5.
[0187] Mathematical formula 1
[0188] Restoration rate (%) = ((thickness of anode composite material layer after vacuum drying (μm) / thickness of anode composite material layer before vacuum drying (μm)) - 1) × 100 (%)
[0189] Mathematical formula 2
[0190] Restoration rate (%) = ((thickness of cathode composite material layer after vacuum drying (μm) / thickness of cathode composite material layer before vacuum drying (μm)) - 1) × 100 (%).
[0191] 2. Moisture content evaluation
[0192] As shown in Tables 3 to 5 below, the moisture content of the cathode active material and the moisture content of the anode active material were measured for the flexible batteries prepared in Examples and Comparative Examples.
[0193] Experimental Example 2
[0194] As shown in Tables 3 to 5 below, the following physical properties were evaluated for the flexible batteries prepared in Examples and Comparative Examples.
[0195] 1. Crack generation evaluation
[0196] For the flexible batteries prepared by the examples and comparative examples, whether the anode active material and the cathode active material had cracks was evaluated by electronic imaging (Camscope) at a magnification of 120. In this case, the crack generation was indicated as ○ and the non-crack generation was indicated as ×, thereby evaluating the crack generation.
[0197] 2. Resistance-related physical property evaluation
[0198] The flexible batteries prepared in the examples and comparative examples were fully charged under the conditions shown in Table 2 below.
[0199] Table 2
[0200]
[0201] 2-1. Resistance measurement
[0202] The resistance of the flexible batteries prepared in the examples and comparative examples was measured using an AC-IR meter. In this case, the resistance value of the flexible battery of Example 1 is 100, and the ratio of the resistance values of the other examples and comparative examples is shown.
[0203] 2-2. Evaluation of resistance change rate after bending in one direction
[0204] For the flexible batteries prepared by the embodiments and comparative examples, under the environmental conditions of temperature of 25°C and humidity of 65%, for the fully charged flexible batteries, the batteries were folded at 1 / 2 position along the length direction and a hydraulic cylinder was used to apply 0.8 kN / 24 cm 2 The film was bent (Bending) within the range of R25 to R38 and then unfolded again. The resistance was then measured for 120 seconds. After the measurement, the resistance was measured at 120 seconds, and then the resistance change rate relative to the resistance before bending was measured.
[0205] 2-3. Evaluation of resistance change rate after bending in two directions
[0206] For the flexible batteries prepared by the embodiments and comparative examples, under the environmental conditions of temperature of 25°C and humidity of 65%, for the fully charged flexible batteries, the batteries were folded at 1 / 2 position along the length direction and a hydraulic cylinder was used to apply 0.8 kN / 24 cm 2 A load of (=26mm×91.5mm) is applied, thereby bending (Bending) in the range of R25 to R38 and then unfolding it again. Under the same conditions, a load is applied in the opposite direction, thereby bending (Bending) in the range of R25 to R38 and then unfolding it again. Subsequently, the resistance is measured for 120 seconds. After the measurement, the resistance is measured at 120 seconds, and then the resistance change rate relative to the resistance before bending is measured.
[0207] 3. Durability evaluation
[0208] Bending the flexible battery so that its two ends are in contact and then restoring it to its original shape is defined as one set of actions. After performing 500 sets, the appearance of the battery was observed using an optical microscope to evaluate whether there was any abnormality in the electrolyte, whether there was any crack in the external material, and other appearance abnormalities. In the evaluation results, 0 indicates no abnormality, and from 1 to 5, the degree of abnormality gradually becomes more serious.
[0209] 4. Evaluation of crack generation after durability evaluation
[0210] For the flexible batteries prepared by the examples and comparative examples for durability evaluation, electronic imaging (Camscope) was used to evaluate whether the anode active material and the cathode active material had cracks at a magnification of 120. In this case, the crack generation was indicated as ○ and the non-crack generation was indicated as ×, thereby evaluating the crack generation.
[0211] Table 3
[0212]
[0213]
[0214] Table 4
[0215]
[0216] Table 5
[0217]
[0218] As shown in Tables 3 to 5 above, compared with Example 2, Example 5, Example 6, Example 9, Example 10, Example 11 and Comparative Examples 1 to 7 which lack any of the conditions, it can be confirmed that the following effects are simultaneously exhibited in Example 1, Example 3, Example 4, Example 7 and Example 8 which all meet the anode current collector vacuum drying conditions, cathode current collector vacuum drying conditions, solid content of the anode active material forming composition and solid content of the cathode active material forming composition of the present invention, namely, no cracks are generated, resistance is low, resistance change rate after bending in one direction or two directions is low, durability is excellent, and no cracks are generated even after durability evaluation.
[0219] Although one embodiment of the present invention is described above, the concept of the present invention is not limited to the embodiment disclosed in this specification. Ordinary technicians who understand the concept of the present invention can easily derive other embodiments within the same scope of the concept by adding, changing, deleting, and appending structural elements, but this also falls within the scope of the concept of the present invention.
Claims
1. A method for preparing a flexible battery, wherein the flexible battery is formed by sealing an electrode assembly and an electrolyte together with an external material, wherein: The method for preparing the electrode assembly comprises: The step of forming an anode composite material by coating a portion or all of at least one side of an anode current collector with an anode active material forming composition and drying the composition, wherein the solid content of the anode active material forming composition is 65 to 85 weight percent, and the viscosity thereof is 7000 to 17000 cps at a temperature of 25° C., and the anode active material forming composition comprises 0.5 to 1.5 weight parts of a first conductive material comprising spherical carbon black, 0.1 to 1 weight parts of a second conductive material comprising graphite, and 1 to 4 weight parts of polyvinylidene fluoride relative to 100 weight parts of the anode material, wherein the average particle size of the anode material is 3 to 20 μm; The step of preparing the anode by vacuum drying the anode current collector at a temperature of 90 to 170° C. for 8 to 16 hours; The step of forming a cathode composite material by coating a cathode active material forming composition on a part or all of at least one side of the cathode current collector and drying the composition, wherein the cathode active material forming composition has a solid content of 35 to 60 weight percent and a viscosity of 5000 to 15000 cps at a temperature of 25° C.; The cathode is prepared by subjecting the cathode current collector to 8 to 16 small vacuum drying steps at a temperature of 60 to 140° C.; and The step of stacking the anode and the cathode by placing a separation membrane between the anode and the cathode, The recovery rate of the anode composite material calculated by the following mathematical formula 1 is 3.5% or less. The recovery rate of the cathode composite material calculated by the following mathematical formula 2 is 4.5% or less. Mathematical formula 1: Restoration rate (%) = ((thickness of anode composite material layer after vacuum drying (μm) / thickness of anode composite material layer before vacuum drying (μm)) - 1) × 100 (%), Mathematical formula 2: Restoration rate (%) = ((thickness of cathode composite material layer after vacuum drying (μm) / thickness of cathode composite material layer before vacuum drying (μm)) - 1) × 100 (%).
2. The method for preparing a flexible battery according to claim 1, characterized in that: The cathode active material forming composition includes 0.55 to 1.6 parts by weight of the first conductive material and 2.5 to 9 parts by weight of polyvinylidene fluoride relative to 100 parts by weight of the cathode material.
3. The method for preparing a flexible battery according to claim 2, characterized in that: The first conductive material includes spherical carbon black.
4. The method for preparing a flexible battery according to claim 1, characterized in that: The step of forming a pattern for coping with contraction and expansion in the longitudinal direction when the electrode assembly is bent may also be included.
5. A flexible battery, characterized in that: include: An electrode assembly, comprising an anode, a cathode and a separation membrane, wherein the anode is coated with an anode active material on a part or all of at least one side of the anode current collector, the cathode is coated with a cathode active material on a part or all of at least one side of the cathode current collector, and the separation membrane is arranged between the anode and the cathode; Electrolyte; as well as The external material is used to seal the electrode assembly and the electrolyte together. The water content of the cathode active material is less than 150 ppm. The water content of the anode active material is 450 ppm or less. The anode active material is formed by an anode active material forming composition, the solid content of the anode active material forming composition is 65 to 85 weight percent, the viscosity is 7000 to 17000 cps at a temperature of 25° C., and, relative to 100 parts by weight of the anode material, the anode active material forming composition comprises 0.5 to 1.5 parts by weight of a first conductive material comprising spherical carbon black, 0.1 to 1 parts by weight of a second conductive material comprising graphite, and 1 to 4 parts by weight of polyvinylidene fluoride, wherein the average particle size of the anode material is 3 to 20 μm; The cathode active material is formed by a cathode active material forming composition, the solid content of the cathode active material forming composition is 35 to 60 weight percent, and the viscosity is 5000 to 15000 cps at a temperature of 25° C.; The resistance change rate measured by the following measurement method 1 is less than 5%, Determination method 1 In a fully charged flexible battery, the battery was bent in the longitudinal direction and then bent in the opposite direction to measure the resistance, and then the resistance change rate relative to the resistance before bending was measured.
6. The flexible battery according to claim 5, characterized in that: The layer thickness of the anode active material is 40 to 60 μm. The layer thickness of the cathode active material is 50 to 75 μm.
7. The flexible battery according to claim 5, characterized in that: The cathode active material forming composition comprises a cathode material, a first conductive material and polyvinylidene fluoride, The average particle size of the cathode material is 8 to 40 μm.
8. The flexible battery according to claim 5, characterized in that: The electrode assembly includes a pattern for coping with contraction and expansion in the longitudinal direction when bent.
9. An auxiliary battery, characterized in that: include: The flexible battery according to any one of claims 5 to 8; as well as A soft shell is used to cover the surface of the above external materials. The housing includes at least one terminal portion for electrically connecting to a device to be charged.