A system and method for refining the surface crystal of aluminum-plated steel strip

By spraying fine aluminum powder on the surface of the aluminum-plated strip, the crystal core is provided to solve the problem of large crystal flowers on the surface of the aluminum-plated plate, improving aesthetics and corrosion resistance, and extending the service life.

CN112048692BActive Publication Date: 2024-11-26TANGSHAN IRON & STEEL GROUP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010858015.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-24
Publication Date
2024-11-26
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

The thick crystal flower coating on the surface of the aluminum plate affects the aesthetics and corrosion resistance of the product, shortening the service life.

Method used

A crystal flower refining system on the surface of aluminum-plated strip steel is designed. Aluminum powder with a particle size of 0.04-0.05mm is sprayed on the surface of the high-temperature aluminum plate by spraying aluminum powder box to provide a large number of crystal cores to promote the refinement of crystal flower.

Benefits of technology

Significantly reduce the crystal flower size on the surface of the aluminum plated plate, beautify the surface, enhance corrosion resistance, and extend service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112048692B_ABST
    Figure CN112048692B_ABST
Patent Text Reader

Abstract

The present invention relates to a system and method for refining crystal flowers on the surface of aluminum-plated steel strip, and belongs to the technical field of hot-dip aluminum-plating equipment in the metallurgical industry. The technical scheme is: an aluminum powder spraying box (3) is arranged above an aluminum pot (4), and the aluminum powder spraying box (3) is provided with a steel strip channel (31) that runs through the aluminum powder spraying box (3) from bottom to top; one end of a smoke exhaust duct (5), an air inlet duct (6) and a return air duct (7) are respectively connected to the aluminum powder spraying box (3), the other end of the air inlet duct (6) is connected to the air outlet of an aluminum powder circulating fan (10), and the other end of the return air duct (7) is connected to the air inlet of the aluminum powder circulating fan (10). The beneficial effect of the present invention is that by spraying extremely fine aluminum powder on the surface of a high-temperature aluminum-plated plate out of the pot, a crystal nucleation core is provided for it, thereby making the crystal flowers on the surface of the aluminum-plated plate more numerous and finer, making the surface of the steel strip more beautiful, and greatly enhancing the corrosion resistance of the aluminum-plated plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a surface crystal flower refinement system and refinement method of aluminum-plated strip steel, belonging to the technical field of hot-dip aluminum-plating equipment in the metallurgical industry. Background Art

[0002] Hot-dip aluminum coating technology has attracted much attention due to its low price, high high-temperature oxidation resistance, and the ability to maintain the original reflectivity at high temperatures. Aluminum-coated plates are mostly used in hot stamping processes, mainly manufacturing heat exchangers, heating gas stoves, stove and oven linings, toaster ovens, and automotive exhaust systems and structural parts. Hot-dip aluminum coating equipment has been put into use in major steel companies across the country, but the coarse crystals on the surface of the aluminum-coated plate not only affect the appearance of the product, but also reduce the corrosion resistance of the aluminum-coated plate and shorten the service life of the aluminum-coated plate. The problem of coarse crystals on the surface of the aluminum-coated plate needs to be solved urgently. Summary of the invention

[0003] The purpose of the present invention is to provide a system and method for refining the surface crystal flowers of aluminum-plated steel strips, which can greatly reduce the size of the crystal flowers on the surface of the steel strip coating, beautify the surface of the steel strip, and solve the problems existing in the background technology.

[0004] The technical solution of the present invention is:

[0005] A surface crystal refinement system for aluminum-plated steel strips, comprising a pyrometer, an aluminum powder spraying box, an aluminum pot, a smoke exhaust duct, an air inlet duct, a return air duct, an aluminum powder spraying device, an aluminum powder circulation fan, a smoke exhaust fan, an aluminum powder rotary filter, an aluminum powder feeder, a ventilator, a steel strip passage, a powder spraying hole and a safety door, wherein the aluminum powder spraying box is arranged above the aluminum pot, the aluminum powder spraying box is provided with a steel strip passage that runs through the aluminum powder spraying box body from bottom to top, and the high-temperature aluminum-plated plate coming out of the aluminum pot passes through the steel strip passage, the steel strip passage is U-shaped, and the aluminum powder spraying box bodies on both sides of the steel strip passage are respectively provided with evenly arranged powder spraying holes, and the opening end of the U-shaped steel strip passage is provided with a safety door, and the safety door is hinged on the aluminum powder spraying box body;

[0006] The inlet and outlet of the steel channel are respectively provided with a ventilator for cooling the high-temperature aluminum-plated plate and a pyrometer for measuring the temperature of the high-temperature aluminum-plated plate;

[0007] One end of the smoke exhaust duct, the air inlet duct and the return air duct are respectively connected to the aluminum powder spraying box, the other end of the smoke exhaust duct is connected to the inlet of the aluminum powder rotary filter through the smoke exhaust fan, the other end of the air inlet duct is connected to the air outlet of the aluminum powder circulating fan, the other end of the return air duct is connected to the air inlet of the aluminum powder circulating fan, the outlet of the aluminum powder rotary filter and the aluminum powder spraying device are respectively connected to the return air duct, and the aluminum powder spraying device is provided with an aluminum powder feeder.

[0008] The spraying directions of the powder spraying holes evenly arranged on the aluminum powder spraying box body on both sides of the strip steel channel are toward the two surfaces of the high-temperature aluminum-plated plates.

[0009] The smoke exhaust duct and the return air duct are respectively provided with air volume control valves.

[0010] The smoke exhaust duct, the air inlet duct and the return air duct are respectively connected to the aluminum powder spraying box through separators.

[0011] The aluminum pot, aluminum powder spraying device, aluminum powder rotary filter, aluminum powder feeder, ventilator and separator in the above-mentioned aluminum-plated strip surface crystal refinement system are all well-known technologies in the art.

[0012] A method for refining crystal flowers on the surface of aluminum-plated steel strips adopts the above-defined system for refining crystal flowers on the surface of aluminum-plated steel strips. The high-temperature aluminum-plated plate coming out of the aluminum pot is cooled by a ventilator and then enters the strip steel channel of the aluminum powder spraying box body. At the same time, the aluminum powder enters the aluminum powder spraying box through the air inlet duct. The powder spraying holes on both sides of the aluminum powder spraying box body spray the aluminum powder evenly onto the surface of the high-temperature aluminum-plated plate. The aluminum powder provides a crystal nucleation core for the high-temperature aluminum-plated plate, thereby making the crystal flowers on the surface of the aluminum-plated plate more numerous and finer.

[0013] The aluminum powder particle size is 0.04-0.05 mm, and the aluminum powder concentration inside the aluminum powder spray box is about 300 to 500 mg / m 3 The temperature of the high-temperature aluminum plate at the entrance of the steel channel is 610℃--630℃.

[0014] The aluminum powder is 325 mesh and has a particle size of 0.045 mm.

[0015] In a supercooled liquid, not all crystal embryos can be transformed into crystal nuclei. Only some crystal embryos with a size larger than a certain critical value can exist stably and grow spontaneously. Such crystal embryos with a size greater than or equal to a certain critical value are crystal nuclei. Under certain supercooling conditions, the free energy of the solid phase is lower than the free energy of the liquid phase. Therefore, when crystal embryos appear in a supercooled liquid, the atoms change from a liquid state to a solid state, which reduces the free energy of the system. This is the driving force for crystallization. At the same time, the crystal embryos form a new surface, forming surface energy, which in turn increases the free energy of the system. This is the resistance to crystallization. If the volume of the crystal embryo is V, the surface area is S, and the unit volume free energy difference between the solid and liquid phases is G γ , the surface free energy per unit area is σ, then the total change in free energy of the system is: △G γ =V△G γ +Sσ. V△G γ is the change in volume free energy caused by the appearance of a crystal embryo in a liquid, and Sσ is the change in surface energy caused by the appearance of a crystal embryo in a liquid. γThe larger the absolute value, the more favorable it is for crystallization. The smaller the absolute value of Sσ, the more favorable it is for crystallization. Assuming there is a spherical embryo with a radius of r in the supercooled liquid, the free energy change caused by it is: △G γ = (4 / 3)πr 3 △G γ +4πr2σ. Its volume free energy change is proportional to the cube of the embryo radius, but the surface energy change is proportional to the square of the radius. The total free energy is the algebraic sum of the volume free energy and the surface free energy. The volume free energy decreases with the cube of r, and the surface energy increases with the square of r. When r increases, the volume free energy decreases faster than the surface energy increases. But at the beginning, the surface energy is dominant. When r increases to a certain critical value, the volume energy is dominant, and the crystal culture can grow spontaneously at this time.

[0016] After many experiments, it was found that 0.045mm aluminum powder particles can grow spontaneously in the crystal culture of 610 to 630 degrees aluminum liquid, which makes the aluminum liquid crystal more numerous and the surface crystal flowers finer. The solidification process of the aluminum liquid on the surface of the strip after it leaves the aluminum pot is non-uniform solidification, and the aluminum flowers on the surface of the aluminum-plated strip are refined by increasing the number of crystal nuclei on the surface of the strip.

[0017] The beneficial effect of the present invention is as follows: the present invention is applied above the hot-dip aluminum-plating pot, and extremely fine aluminum powder is sprayed onto the surface of the high-temperature aluminum-plated plate coming out of the pot to provide a nucleus for the nucleation of the crystal, thereby making the crystal flowers on the surface of the aluminum-plated plate more numerous and finer, making the surface of the strip more beautiful, and greatly enhancing the corrosion resistance of the aluminum-plated plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the present invention;

[0019] Figure 2 This is a front view of the aluminum powder spraying box of the present invention;

[0020] Figure 3 This is a side view of the aluminum powder spraying box of the present invention;

[0021] Figure 4 This is a top view of the aluminum powder spraying box of the present invention;

[0022] Figure 5 This is a main sectional view of the aluminum powder spraying box of the present invention;

[0023] Figure 6 This is a photo of the aluminum plate before spraying aluminum powder;

[0024] Figure 7 This is a photo of the aluminum plate after spraying aluminum powder;

[0025] Figure 8 It is the experimental data graph of the cyclic salt spray experiment;

[0026] In the figure: pyrometer 1, cooling fan 2, aluminum powder spraying box 3, aluminum pot 4, exhaust duct 5, air inlet duct 6, return air duct 7, air volume control valve 8, aluminum powder spraying device 9, aluminum powder circulation fan 10, exhaust fan 11, aluminum powder rotary filter 12, aluminum powder feeder 13, ventilator 14, separator 15, strip steel channel 31, powder spraying hole 32, safety door 33. DETAILED DESCRIPTION

[0027] The present invention will be further described below by way of examples with reference to the accompanying drawings.

[0028] Refer to the attached Figure 1-5 , a surface crystal flower refinement system of aluminum-plated steel strip, comprising a pyrometer 1, an aluminum powder spraying box 3, an aluminum pot 4, a smoke exhaust duct 5, an air inlet duct 6, a return air duct 7, an aluminum powder spraying device 9, an aluminum powder circulation fan 10, a smoke exhaust fan 11, an aluminum powder rotary filter 12, an aluminum powder feeder 13, a ventilator 14, a steel strip channel 31, a powder spraying hole 32 and a safety door 33, the aluminum powder spraying box 3 is arranged above the aluminum pot 4, the aluminum powder spraying box 3 is provided with a steel strip channel 31 which runs through the aluminum powder spraying box 3 box body from bottom to top, and the high-temperature aluminum-plated plate coming out of the aluminum pot 4 passes through the steel strip channel 31, the steel strip channel 31 is U-shaped, and the aluminum powder spraying box 3 boxes on both sides of the steel strip channel 31 are respectively provided with evenly arranged powder spraying holes 32, and the opening end of the U-shaped steel strip channel 31 is provided with a safety door 33, and the safety door 33 is hinged on the aluminum powder spraying box 3 box body;

[0029] The inlet and outlet of the strip steel channel 31 are respectively provided with a ventilator 14 for cooling the high-temperature aluminum-plated plate and a pyrometer 1 for measuring the temperature of the high-temperature aluminum-plated plate;

[0030] One end of the smoke exhaust duct 5, the air inlet duct 6 and the return air duct 7 are respectively connected to the aluminum powder spraying box 3, the other end of the smoke exhaust duct 5 is connected to the inlet of the aluminum powder rotary filter 12 through the smoke exhaust fan 11, the other end of the air inlet duct 6 is connected to the air outlet of the aluminum powder circulating fan 10, the other end of the return air duct 7 is connected to the air inlet of the aluminum powder circulating fan 10, the outlet of the aluminum powder rotary filter 12 and the aluminum powder spraying device 9 are respectively connected to the return air duct 7, and the aluminum powder spraying device 9 is provided with an aluminum powder feeder 13.

[0031] In this embodiment, refer to the attached Figure 1 The aluminum pot 4, the aluminum powder spraying device 9, the aluminum powder rotary filter 12, the aluminum powder feeder 13, the ventilator 14 and the separator 15 are all well-known technologies in the art, wherein:

[0032] The aluminum powder rotary filter 12 is a rotary filter, and its filter element rotates once every 100 to 120 seconds. There are four filter elements in total. The aluminum powder in the smoke exhaust duct is filtered by one filter element and the clean gas is discharged into the factory. The other three filter elements blow air in the reverse direction to transport the aluminum powder back to the return air duct for recycling.

[0033] The aluminum powder feeder 13 is produced by Sanang Machinery Co., Ltd. and its model is LX-300MM. Every 10% opening can deliver about 70 grams of aluminum powder per hour to the aluminum powder spraying box.

[0034] The fan 14 is a cooling device produced by Weihai Weili Fan Co., Ltd., and its model is: WFG-1450D JB / T10563-2006.

[0035] The separator 15 is a pipeline connection device commonly used in the art.

[0036] Refer to the attached Figure 1-5 The aluminum powder spraying box 3 is provided with a strip steel channel 31 which runs through the aluminum powder spraying box 3 from bottom to top. The high-temperature aluminum-plated plate coming out of the aluminum pot 4 passes through the strip steel channel 31. The strip steel channel 31 is U-shaped. The aluminum powder spraying box 3 on both sides of the strip steel channel 31 are respectively provided with evenly arranged powder spraying holes 32. A safety door 33 is provided at the open end of the U-shaped strip steel channel 31. The safety door 33 is hinged on the aluminum powder spraying box 3.

[0037] Aluminum powder spraying device 9 is installed behind aluminum powder feeder 13, and aluminum powder spraying device 9 transports aluminum powder to return air duct 7, and circulating fan 10 allows aluminum powder to enter air inlet duct 6 and finally enter aluminum powder spraying box 3. Smoke exhaust fan 11 continuously extracts excess aluminum powder to rotary filter 12 through exhaust duct 5, so that negative pressure is formed in aluminum powder spraying box 3, air inlet duct 6 and return air duct 7. The filter element of rotary filter rotates once every 100 to 120 seconds, and there are four filter elements in total. After aluminum powder in the exhaust duct is filtered by one filter element, clean gas is discharged into the factory building, and the other three filter elements blow air in the opposite direction, and the aluminum powder therein is transported back to return air duct 7 for recycling.

[0038] The aluminum powder spraying box 3 and the cooling fan 2 and the ventilator 14 below it are installed on a mobile fan platform, which is moved out from above the aluminum pot 4 when the machine is parked. The aluminum powder spraying box 3 is connected to the three pipes through the air inlet pipe separator, the return air pipe separator, and the exhaust pipe separator. The pyrometer 1 is installed at the entrance of the strip steel channel 31 of the aluminum powder spraying box 3 to observe the temperature of the strip steel in the aluminum powder spraying box 3 at all times and adjust it through the fan below it.

[0039] The return air duct 7 and the smoke exhaust duct 5 are installed with air volume control valves 8 to control the air volume inside them.

[0040] The system is installed above the aluminum pot 4 and sprays extremely fine aluminum powder onto the high-temperature coating. The aluminum powder uses 325 mesh and 0.045mm particle size products produced by Hunan Jintian High-Tech Co., Ltd. After the fine aluminum powder is sprayed into the molten aluminum layer, it provides a large number of crystal nucleation cores.

[0041] After the strip steel leaves the aluminum pot, it passes through the ventilator 14 and enters the aluminum powder spraying box 3, then enters the ventilator 14 for cooling, and finally enters the water quenching tank through the turning roller. The aluminum powder concentration inside the aluminum powder spraying box 3 is about 300 to 500 mg / m 3 .

[0042] The type of steel produced in this embodiment is DC51D with a yield strength of 150 MPa to 230 MPa, ordinary carbon steel, with a width of 1250 mm, a thickness of 1 mm, and a production line speed of 110 m / min.

[0043] Preparation: Before spraying aluminum powder, add sufficient aluminum powder to the aluminum powder feeder 13 with a special stainless steel shovel, and go to the site to confirm whether the safety door 33 of the aluminum powder spraying box 3 and the air inlet duct separator, return air duct separator, and exhaust duct separator are open, and adjust the control mode of each device from local mode to remote mode.

[0044] A. Specific steps for starting the machine:

[0045] (1) Move the mobile fan platform to the working position above the aluminum pot 4.

[0046] (2) Close the air inlet duct separator, return air duct separator, and exhaust duct separator, and connect these three ducts to the aluminum powder spraying box;

[0047] (3) Close the safety door 33 of the aluminum powder spraying box 3;

[0048] (4) Adjust the opening of the fan below the aluminum powder box 3 so that the inlet temperature of the strip channel 31 of the aluminum powder box 3 is 620-530.628°C, and adjust the opening of the fan above the aluminum powder box 3 so that the temperature of the strip after exiting the strip channel 31 and being cooled by the cooling fan above the aluminum powder box 3 is below 270°C;

[0049] (5) Turn on the aluminum powder exhaust fan, set the opening to 50%, the speed to 750 rpm, and the air volume control valve opening to 70 to ensure that the pressure in the aluminum powder box 3 is negative pressure;

[0050] (6) Turn on the aluminum powder circulation fan, set the opening to 65%, the speed to 975 rpm, and the air volume control valve opening to 70;

[0051] (7) Turn on the aluminum powder spraying device 9, adjust the power of the aluminum powder feeder 13 to 50%, set the opening of the feeding fan to 75%, and the speed to 1125 rpm;

[0052] (8) The aluminum powder rotary filter 12 is operated, and the cycle period is set to one filter element rotation every 120 seconds.

[0053] B. Specific steps for shutdown operation:

[0054] (1) Close the aluminum powder feeder 13 to stop the supply of aluminum powder;

[0055] (2) Turn off the aluminum powder spraying device 9 and stop conveying the remaining aluminum powder into the pipeline;

[0056] (3) closing the aluminum powder rotary filter 12;

[0057] (4) Turn off the aluminum powder circulation fan and air volume control valve;

[0058] (5) Turn off the aluminum powder exhaust fan;

[0059] (6) Turn off all strip cooling fans;

[0060] (7) Open the safety door 33 of the aluminum powder spraying box 3 so that the aluminum powder spraying box 3 will not scrape the strip when it is removed;

[0061] (8) Open the air inlet duct separator, the return air duct separator, and the smoke exhaust duct separator, and cut off the connection between the aluminum powder box 3 and the duct;

[0062] (9) Move the mobile fan platform loaded with the aluminum powder spraying box 3 to the parking space, free up the space above the aluminum pot 4, and lift out the air knife and three-roller six-arm in the aluminum pot 4.

[0063] Through the comparison of cyclic salt spray test, it was found that the average time for red rust to appear on the surface of 1mm thick aluminum plate after passivation treatment increased from 721 hours to 769 hours. The experimental data is shown in Figure 8 .

[0064] The experimental method of this cyclic salt spray test is 2 hours of 5% sodium chloride salt spray treatment, 4 hours of 60 degrees drying treatment, 2 hours of water atomization treatment, 8 hours as a cycle, continuous corrosion of the sample, observe and record the time when the sample appears red rust. In addition, spraying aluminum powder on the surface of the strip can also improve minor defects such as missing plating and scratches.

Claims

1. A system for refining the surface of aluminum-plated steel strip, characterized by: The invention comprises a pyrometer (1), an aluminum powder spraying box (3), an aluminum pot (4), a smoke exhaust duct (5), an air inlet duct (6), a return air duct (7), an aluminum powder spraying device (9), an aluminum powder circulation fan (10), a smoke exhaust fan (11), an aluminum powder rotary filter (12), an aluminum powder feeder (13), a ventilator (14), a steel strip channel (31), a powder spraying hole (32) and a safety door (33). The aluminum powder spraying box (3) is arranged above the aluminum pot (4). (3) A strip steel channel (31) is provided which runs through the aluminum powder spraying box (3) from bottom to top, and the high-temperature aluminum-plated plate coming out of the aluminum pot (4) passes through the strip steel channel (31). The strip steel channel (31) is U-shaped, and the aluminum powder spraying box (3) on both sides of the strip steel channel (31) is provided with evenly arranged powder spraying holes (32). A safety door (33) is provided at the open end of the U-shaped strip steel channel (31), and the safety door (33) is hinged on the aluminum powder spraying box (3); The inlet and outlet of the strip steel channel (31) are respectively provided with a ventilator (14) for cooling the high-temperature aluminum-plated plate and a pyrometer (1) for measuring the temperature of the high-temperature aluminum-plated plate; One end of the smoke exhaust duct (5), the air inlet duct (6) and the return air duct (7) are respectively connected to the aluminum powder spraying box (3); the other end of the smoke exhaust duct (5) is connected to the inlet of the aluminum powder rotary filter (12) through the smoke exhaust fan (11); the other end of the air inlet duct (6) is connected to the air outlet of the aluminum powder circulation fan (10); the other end of the return air duct (7) is connected to the air inlet of the aluminum powder circulation fan (10); the outlet of the aluminum powder rotary filter (12) and the aluminum powder spraying device (9) are respectively connected to the return air duct (7); and the aluminum powder spraying device (9) is provided with an aluminum powder feeder (13).

2. The system for surface crystal refinement of aluminum-plated steel strip according to claim 1, characterized in that: The spraying directions of the powder spraying holes (32) evenly arranged on the box body of the aluminum powder spraying box (3) on both sides of the strip steel channel (31) are toward the two surfaces of the high-temperature aluminum-plated plate.

3. The surface crystal refinement system of aluminum-plated steel strip according to claim 1 is characterized in that: The smoke exhaust duct (5) and the return air duct (7) are respectively provided with air volume control valves (8).

4. The system for refining the surface crystals of aluminum-plated steel strip according to claim 1, characterized in that: The smoke exhaust duct (5), the air inlet duct (6) and the return air duct (7) are respectively connected to the aluminum powder spraying box (3) via separators (15).

5. A method for refining the surface crystals of aluminum-plated steel strip, characterized in that: A system for refining the surface crystals of aluminum-plated strip steel as defined in any one of claims 1 to 4 is used. The high-temperature aluminum-plated plate coming out of the aluminum pot (4) is cooled by a ventilator (14) and then enters the strip steel channel (31) of the aluminum powder spraying box (3). At the same time, aluminum powder enters the aluminum powder spraying box (3) through the air inlet duct (6). The powder spraying holes (32) on both sides of the aluminum powder spraying box (3) spray the aluminum powder evenly onto the surface of the high-temperature aluminum-plated plate. The aluminum powder provides a crystal nucleation core for the high-temperature aluminum-plated plate, thereby making the surface crystals of the aluminum-plated plate more numerous and finer.

6. The method for refining the surface crystals of aluminum-plated steel strip according to claim 5, characterized in that: The aluminum powder particle size is 0.04-0.05 mm, and the aluminum powder concentration inside the aluminum powder spraying box (3) is 300 to 500 mg / m 3 The temperature of the high temperature aluminum plate at the entrance of the strip steel channel (31) is 610°C - 630°C.

7. The method for refining the surface crystals of aluminum-plated steel strip according to claim 6, characterized in that: The aluminum powder is 325 mesh and has a particle size of 0.045 mm.