A glass passivated solid package low voltage diode and its manufacturing method
By synchronizing the PN junction during the welding process of the electrode leads of the glass passivation solid package diode and the die, the short circuit problem caused by insufficient depth of PN junction in traditional processes is solved, and the production of diodes below 6V is achieved, ensuring high voltage Output.
Patent Information
- Application Number
- CN202011060738.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Traditional manufacturing processes are difficult to obtain glass passivated solid packaged diodes below 6V, because the depth of the PN junction in the die is too shallow, causing welding metal to pass through the PN junction, causing short circuits, and the production of low-voltage diodes cannot be achieved.
By synchronously forming PN junctions during welding between the electrode leads and the die, the PN junctions are avoided redistribution due to high temperature processes. The alloy welding technology of silicon wafers, aluminum sheets and electrode leads is used to form a sudden junction to increase the diode voltage, ensuring that The PN junction depth is above 20μm, ensuring that the welded metal does not pass through the PN junction.
A glass passivation solid package diode below 6V was successfully manufactured, which avoided the voltage reduction problem caused by PN junction short circuit in traditional processes and achieved a higher diode voltage output.
Smart Images

Figure CN112186044B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a glass passivation solid package low-voltage diode and a manufacturing method thereof, belonging to the technical field of diodes. Background Art
[0002] Glass passivated solid packaged diodes are widely used in mid-to-high-end fields due to their small size, good high-temperature stability, strong radiation resistance, high reliability, and low cost. However, traditional manufacturing processes such as diffusion, epitaxy, and ion implantation can only obtain glass passivated solid packaged diodes above 6V, and cannot produce low-voltage diodes below 6V. The main reason is that the low-voltage diode cores below 6V obtained by diffusion, epitaxy, ion implantation and other manufacturing processes have very shallow junction depths, generally less than 5μm, in order to obtain a large concentration gradient. However, in the subsequent high-temperature welding of leads and glass passivation solid packaging process, the PN junction of the core is too shallow, and during welding and glass passivation, the welding metal will cross the PN junction, resulting in a PN junction short circuit, and a low-voltage glass passivated solid packaged diode below 6V cannot be obtained. Therefore, it is difficult to obtain glass passivated solid packaged diodes below 6V using traditional manufacturing processes. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a glass passivated solid package low voltage diode and a manufacturing method thereof.
[0004] The present invention is achieved through the following technical solutions:
[0005] A glass-passivated solid-package low-voltage diode comprises a silicon wafer A and two electrode leads, wherein the silicon wafer A is located between the two electrode leads, wherein one electrode lead is connected to the silicon wafer A via a welding metal A, and the other electrode lead is connected to the silicon wafer A via a welding metal B, wherein the silicon wafer A, the welding metal A, the welding metal B and the two electrode leads are all arranged in a passivation glass, and one end of the electrode lead extends outside the passivation glass.
[0006] The silicon wafer A is an N-type single crystal silicon wafer, including an N layer and an N+ layer, wherein the N layer is close to the welding metal A, and the N+ layer is close to the welding metal B.
[0007] The electrode lead comprises a copper lead and a molybdenum electrode, and the molybdenum electrode is welded and connected to the copper lead via a silver-copper sheet.
[0008] The welding metal A is an aluminum sheet.
[0009] The aluminum sheet has a thickness of 40 μm-100 μm and a composition of silicon:aluminum=(0-15)%.
[0010] The welding metal B is a vaporized aluminum layer, and the vaporized aluminum layer has a thickness of 6 μm-16 μm.
[0011] A method for manufacturing a glass passivated solid package low-voltage diode comprises the following steps:
[0012] Step 1, preparing a tube core;
[0013] Step 2: high temperature sintering, welding the copper lead and the molybdenum electrode into a complete electrode lead through the silver copper sheet;
[0014] Step 3: vertically stack the electrode lead, the tube core, the aluminum sheet, and the electrode lead in the graphite mold in sequence, and then place the graphite mold in a vacuum sintering furnace to perform fusion welding bonding on the electrode lead, the tube core, and the aluminum sheet;
[0015] Step 4: Insert the diode after welding into the corrosion tray, and use KOH solution with a concentration of 2-12% and a temperature of 80-100°C to corrode it for 3-7 minutes. After corrosion, rinse it with hot deionized water. After rinsing, put the diode into hot deionized water and boil it 3-7 times. Then take out the diode and cross-rinse it with hot and cold deionized water for more than half an hour.
[0016] Step 5: Coat the surface of the diode with glass slurry, and then place it in a high-temperature molding furnace for molding.
[0017] The tube core preparation in step 1 includes the following steps:
[0018] A. Select N-type single crystal silicon wafer with a resistivity of 0.003Ω·cm~0.04Ω·cm;
[0019] B. Place N-type single crystal silicon wafer in the source for phosphorus diffusion to form N+NN+ silicon wafer, with a diffusion junction depth of 10μm~80μm, a sheet resistance of 0.1Ω / □~3Ω / □, and a source ratio of P2O5:C2H5OH=5~6g:50ml;
[0020] C. After phosphorus diffusion, the silicon wafer is ground to remove one side of the N+ layer to form N N+ silicon wafer A, with a thickness of 200μm~350μm;
[0021] D. Aluminum is evaporated on the N+ surface of silicon wafer A. The thickness of the aluminum vaporization layer is 6μm-16μm. After aluminum vaporization, silicon wafer A is placed in a vacuum sintering furnace. Silicon wafer A and the aluminum vaporization layer are fusion-bonded at a temperature of 450-550°C for 5-20 minutes.
[0022] F. Use ultrasonic cutting to split silicon wafer A into the required tube core size, and use a solution with a volume ratio of HF:HNO3=1:5 to corrode the chip obtained by splitting. The corrosion time is 80~180S, and then use cold deionized water to rinse the chip and dry it to obtain the tube core.
[0023] The vacuum degree in the vacuum sintering furnace in step 3 is ≥3.4×10 -3pa, the fusion bonding temperature is 750~790℃, the fusion bonding time is 10min~60min, and the obtained diode is naturally cooled in a vacuum sintering furnace and taken out below 100℃.
[0024] In the step 5, the ratio of the glass powder slurry is glass powder: water = 3g: 1ml, the temperature in the high temperature molding furnace is increased to 650°C within 20-70 minutes, and then the temperature is lowered after being kept constant for 1-8 minutes, and the cooling rate is ≤3°C / min.
[0025] The beneficial effects of the present invention are as follows: the core PN junction of the diode is obtained synchronously during the welding process of the electrode lead and the tube core, thereby avoiding the problem that the PN junction is redistributed due to the high-temperature process, which ultimately leads to a significant increase in the diode voltage, and avoiding the problem that the welding metal crosses the PN junction during welding due to the shallow PN junction depth of the tube core in traditional diodes, resulting in a PN junction short circuit. Glass-passivated solid packaged diodes below 6V can be manufactured. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a structural schematic diagram of a glass passivated solid package low-voltage diode of the present invention;
[0027] Figure 2 It is a schematic diagram of the structure in which the electrode lead, tube core, aluminum sheet, and electrode lead are vertically stacked in sequence in a graphite mold.
[0028] In the figure: 1-copper lead, 2-silver copper sheet, 3-molybdenum electrode, 4-welding metal A, 5-silicon wafer A, 6-passivation glass, 7-welding metal B. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0030] like Figure 1 and Figure 2 As shown, a glass-passivated solid-packaged low-voltage diode described in the present invention includes a silicon wafer A5 and two electrode leads, wherein the silicon wafer A5 is located between the two electrode leads, wherein one electrode lead is connected to the silicon wafer A5 via a welding metal A4, and the other electrode lead is connected to the silicon wafer A5 via a welding metal B7, wherein the silicon wafer A5, the welding metal A4, the welding metal B7 and the two electrode leads are all arranged in a passivation glass 6, and one end of the electrode lead extends outside the passivation glass 6.
[0031] The silicon wafer A5 is an N-type single crystal silicon wafer, including an N layer and an N+ layer, wherein the N layer is close to the welding metal A4, and the N+ layer is close to the welding metal B7.
[0032] The electrode lead comprises a copper lead 1 and a molybdenum electrode 3 , and the molybdenum electrode 3 is welded to the copper lead 1 through a silver-copper sheet 2 .
[0033] The welding metal A4 is an aluminum sheet.
[0034] The aluminum sheet has a thickness of 40 μm-100 μm and a composition of silicon: aluminum = 0-15%.
[0035] The welding metal B7 is a vapor-evaporated aluminum layer, and the thickness of the vapor-evaporated aluminum layer is 6 μm-16 μm.
[0036] A method for manufacturing a glass passivated solid package low-voltage diode comprises the following steps:
[0037] Step 1, preparing a tube core;
[0038] Step 2: high temperature sintering, welding the copper lead 1 and the molybdenum electrode 3 into a complete electrode lead through the silver copper sheet 2;
[0039] Step 3: vertically stack the electrode lead, the tube core, the aluminum sheet, and the electrode lead in the graphite mold in sequence, and then place the graphite mold in a vacuum sintering furnace to perform fusion welding bonding on the electrode lead, the tube core, and the aluminum sheet;
[0040] Step 4: Insert the diode after welding into the corrosion tray, and use KOH solution with a concentration of 2-12% and a temperature of 80-100°C to corrode it for 3-7 minutes. After corrosion, rinse it with hot deionized water. After rinsing, put the diode into hot deionized water and boil it 3-7 times. Then take out the diode and cross-rinse it with hot and cold deionized water for more than half an hour.
[0041] Step 5: Coat the surface of the diode with glass slurry, and then place it in a high-temperature molding furnace for molding.
[0042] The tube core preparation in step 1 includes the following steps:
[0043] A. Select N-type single crystal silicon wafer with resistivity of 0.003Ω·cm~0.04Ω·cm.
[0044] B. Place the N-type single crystal silicon wafer in the source for phosphorus diffusion to form an N+NN+ silicon wafer with a diffusion junction depth of 10μm~80μm and a sheet resistance of 0.1Ω / □~3Ω / □. The source ratio is P2O5:C2H5OH (anhydrous ethanol) = 5~6g:50ml.
[0045] C. After phosphorus diffusion, the silicon wafer is ground to remove one side of the N+ layer to form N N+ silicon wafer A5. The thickness of silicon wafer A5 is 200μm~350μm.
[0046] D. Aluminum is evaporated on the N+ surface of silicon wafer A5, and the thickness of the evaporated aluminum layer is 6μm-16μm. After aluminum is evaporated, silicon wafer A5 is placed in a vacuum sintering furnace, and silicon wafer A5 and the evaporated aluminum layer are fusion-bonded at a temperature of 450~550℃ for 5~20min. When in use, the evaporated aluminum layer is formed on the N+ surface of the chip by electron beam evaporation.
[0047] F. Use ultrasonic cutting to split the silicon wafer A5 into the required tube core size, and use a solution with a volume ratio of HF:HNO3=1:5 to corrode the chip obtained by splitting. The corrosion time is 80~180S, and then use cold deionized water to rinse the chip and dry it to obtain the tube core.
[0048] The vacuum degree in the vacuum sintering furnace in step 3 is ≥3.4×10 -3 pa, the fusion bonding temperature is 750~790℃, the fusion bonding time is 10min~60min, and the obtained diode is naturally cooled in a vacuum sintering furnace and taken out below 100℃.
[0049] In the step 5, the ratio of the glass powder slurry is glass powder: water = 3g: 1ml, the temperature in the high temperature molding furnace is increased to 650°C within 20-70 minutes, and then the temperature is lowered after being kept constant for 1-8 minutes, and the cooling rate is ≤3°C / min.
[0050] Specifically, the process flow of the present invention is single crystal wafer→phosphorus diffusion→grinding→aluminum evaporation→splitting→molding→alloying / welding→table top etching→wave powder coating and molding.
[0051] The junction depth of low-voltage diode tube cores below 6V obtained by traditional manufacturing processes such as diffusion, epitaxy, and ion implantation is very shallow, generally less than 5μm, in order to obtain a large concentration gradient. However, when manufacturing glass-passivated solid packaged diodes, the welding temperature between the tube core and the electrode lead is very high, around 700℃. If the PN junction depth is too shallow, the welding metal will pass through the PN junction during welding, causing the PN junction to short-circuit. In order to avoid the above problems, the PN junction depth of glass-passivated solid packaged diodes is generally controlled to be above 20μm. Therefore, traditional manufacturing methods cannot obtain glass-passivated solid packaged diodes below 6V.
[0052] The present invention provides a glass passivated solid package low-voltage diode and a manufacturing method. The core PN junction of the diode is not formed before the electrode lead and the tube core are "alloyed / welded" (in the traditional manufacturing process, the core PN junction of the diode has been formed before the electrode lead and the tube core are welded). The PN junction of the diode is formed in the "alloyed / welded" process. During the "alloyed / welded", the N surface of the tube core and the aluminum sheet alloy form the core PN junction of the diode. The obtained PN junction is a sudden junction, which can obtain a very low reverse voltage; at the same time, the upper electrode lead is welded to the aluminum sheet, and the lower electrode lead is welded to the tube core through the evaporated aluminum layer on the N+ surface of the tube core. The purpose of manufacturing the N+ layer of the tube core is to enable the tube core to form a good ohmic contact with the electrode lead.
[0053] The core PN junction of the diode is obtained synchronously during the welding process of the electrode lead and the tube core, which avoids the problem of the PN junction being redistributed due to the high-temperature process (the junction depth deepens and the concentration gradient decreases), which ultimately leads to a significant increase in the diode voltage. It also avoids the problem of the traditional diode having a PN junction that is too shallow, and the welding metal crossing the PN junction during welding, causing a PN junction short circuit. Glass-passivated solid packaged diodes below 6V can be manufactured.
[0054] Embodiment 1:
[0055] The manufacturing process and process method of 2V / 0.5W Zener diode are as follows:
[0056] Single crystal wafer→ Phosphorus diffusion→ Grinding→ Aluminum steaming→ Splitting→ Molding→ Alloying / welding→ Tabletop etching→ Powder coating and molding
[0057] 1. Single crystal: Use N-type single crystal silicon wafer with a resistivity of 0.008Ω·cm -0.009·cm.
[0058] 2. Phosphorus diffusion: The source ratio is P2O5: C2H5OH (anhydrous ethanol) = 5~6g: 50ml. The silicon wafer is immersed in the source. The diffusion time is 25h; the diffusion temperature is 1280±2℃; the diffusion junction depth is 40±5μm; the sheet resistance is 0.1Ω / □~0.3Ω / □.
[0059] 3. Grinding: Grind one side. The thickness of the silicon wafer after grinding is 250±10μm.
[0060] 4. Aluminum steaming: Aluminum is steamed on the retained phosphorus diffusion surface (fine grinding surface is not steamed with aluminum), and the thickness of the aluminum layer is 11μm; after aluminum steaming, the alloy is alloyed, the alloy temperature is 500±10℃, and the constant temperature time is 5~10min.
[0061] 5. Splitting: Use ultrasonic cutting to split large pieces into Ф1.5 tube cores. The split chips are placed in HF:HNO3=1:5 (volume ratio) for corrosion, and the corrosion time is 80~110S; rinse with a large amount of cold deionized water and then dry.
[0062] 6. Mold assembly: Press the electrode lead, tube core, and aluminum sheet Figure 2 Assembled in a graphite mold. The diameter of the molybdenum electrode 3 is Φ1.5; the diameter of the copper lead 1 is Φ0.8, the composition of the aluminum sheet is silicon: aluminum = 5%, and the thickness of the aluminum sheet is 80μm.
[0063] 7. Alloy / welding: Vacuum degree: ≥3.4X10 -3 pa, temperature: 750~760℃, time: 20min~30min, naturally cool down to 450℃, the diode can be taken out when the temperature is below 100℃.
[0064] 8. Countertop corrosion: Place the diode in a 5% KOH solution at 90°C for 5 minutes, take it out and rinse it with hot deionized water, boil it in hot deionized water for 5 times, and cross-rinse it with hot and cold deionized water for more than half an hour.
[0065] 9. Glass powder coating molding: The ratio of glass slurry is glass powder: water = 3g: 1ml. The product is completely coated with glass powder. High temperature molding: 20~70 min to heat up to the maximum temperature of 650℃, maintain for 2min, and the cooling rate is ≤3℃ / min.
[0066] Embodiment 2:
[0067] The manufacturing process and process method of 5V / 0.5W Zener diode are as follows:
[0068] Single crystal wafer→ Phosphorus diffusion→ Grinding→ Aluminum steaming→ Splitting→ Molding→ Alloying / welding→ Tabletop etching→ Powder coating and molding
[0069] 1. Single crystal wafer: Use N-type single crystal silicon wafer with a resistivity of 0.019~0.020Ω·cm.
[0070] 2. Phosphorus diffusion: The source ratio is P2O5: C2H5OH (anhydrous ethanol) = 5~6g: 50ml. The silicon wafer is immersed in the source. The diffusion time is 22h; the diffusion temperature is 1280±2℃; the diffusion junction depth is 40±5μm; the sheet resistance is 0.1Ω / □~0.3Ω / □.
[0071] 3. Grinding: Grind one side. The thickness of the silicon wafer after grinding is 250±10μm.
[0072] 4. Aluminum steaming: Aluminum is steamed on the retained phosphorus diffusion surface (fine grinding surface is not steamed), and the thickness of the aluminum layer is 12μm; after aluminum steaming, the alloy is alloyed, the alloy temperature is 500±10℃, and the constant temperature time is 5~10min.
[0073] 5. Splitting: Use ultrasonic cutting to split large pieces into Ф1.5 tube cores. The split chips are placed in HF:HNO3=1:5 (volume ratio) for corrosion, and the corrosion time is 80~110S; rinse with a large amount of cold deionized water and then dry.
[0074] 6. Mold assembly: Press the electrode lead, tube core, and aluminum sheet Figure 2 Assembled in a graphite mold. The diameter of the molybdenum electrode 3 is Φ1.5; the diameter of the copper lead 1 is Φ0.8, the composition of the aluminum sheet is silicon: aluminum = 5%, and the thickness of the aluminum sheet is 80μm.
[0075] 7. Alloy / welding: Vacuum degree: ≥3.4X10 -3 pa, temperature: 750~760℃, time: 20min~30min, naturally cool down to 450℃, the diode can be taken out when the temperature is below 100℃.
[0076] 8. Countertop corrosion: Place the diode in a 5% KOH solution at 95°C for 5 minutes, take it out and rinse it with hot deionized water, boil it in hot deionized water for 5 times, and cross-rinse it with hot and cold deionized water for more than half an hour.
[0077] 9. Glass powder coating molding: The ratio of glass slurry is glass powder: water = 3g: 1ml. The product is completely coated with glass powder. High temperature molding: heat up to the maximum temperature of 650℃ for 20~70 min, maintain for 1~3 min, and the cooling rate is ≤3℃ / min.
[0078] Embodiment three:
[0079] The manufacturing process and process method of 2V / 2W Zener diode are as follows:
[0080] Single crystal wafer→ Phosphorus diffusion→ Grinding→ Aluminum steaming→ Splitting→ Molding→ Alloying / welding→ Tabletop etching→ Powder coating and molding
[0081] 1. Single crystal wafer: Use N-type single crystal silicon wafer with a resistivity of 0.008Ω·cm~0.009Ω·cm.
[0082] 2. Phosphorus diffusion: The source ratio is P2O5: C2H5OH (anhydrous ethanol) = 5~6g: 50ml. The silicon wafer is immersed in the source. The diffusion time is 25h; the diffusion temperature is 1280±2℃; the diffusion junction depth is 40±5μm; the sheet resistance is 0.1Ω / □~0.3Ω / √.
[0083] 3. Grinding: Grind one side. The thickness of the silicon wafer after grinding is 250±10μm.
[0084] 4. Aluminum steaming: Aluminum is steamed on the retained phosphorus diffusion surface (fine grinding surface is not steamed with aluminum), and the thickness of the aluminum layer is 11μm; after aluminum steaming, the alloy is alloyed, the alloy temperature is 500±10℃, and the constant temperature time is 5~10min.
[0085] 5. Splitting: Use ultrasonic cutting to split large pieces into Ф2 tube cores. The split chips are placed in HF:HNO3=1:5 (volume ratio) for corrosion, and the corrosion time is 80~110S; rinse with a large amount of cold deionized water and then dry.
[0086] 6. Mold assembly: Press the electrode lead, tube core, and aluminum sheet Figure 2 Assembled in a graphite mold. The diameter of the molybdenum electrode 3 is Φ2; the diameter of the copper lead 1 is Φ1.2, the composition of the aluminum sheet is silicon: aluminum = 5%, and the thickness of the aluminum sheet is 85μm.
[0087] 7. Alloy / welding: Vacuum degree: ≥3.4X10 -3 pa, temperature: 750~760℃, time: 30min~40min, naturally cool down to 450℃, the diode can be taken out below 100℃.
[0088] 8. Countertop corrosion: Place the diode in a 5% KOH solution at 90°C for 5 minutes, take it out and rinse it with hot deionized water, boil it in hot deionized water for 5 times, and cross-rinse it with hot and cold deionized water for more than half an hour.
[0089] 9. Glass powder coating molding: The ratio of glass slurry is glass powder: water = 3g: 1ml. The product is completely coated with glass powder. High temperature molding: 20~70 min to heat up to the maximum temperature of 650℃, maintain for 2min, and the cooling rate is ≤3℃ / min.
[0090] Embodiment 4:
[0091] The manufacturing process and process method of 5V / 2W Zener diode are as follows:
[0092] Single crystal wafer→ Phosphorus diffusion→ Grinding→ Aluminum steaming→ Splitting→ Molding→ Alloying / welding→ Tabletop etching→ Powder coating and molding
[0093] 1. Single crystal wafer: Use N-type single crystal silicon wafer with a resistivity of 0.019~0.020Ω·cm.
[0094] 2. Phosphorus diffusion: The source ratio is P2O5: C2H5OH (anhydrous ethanol) = 5~6g: 50ml. The silicon wafer is immersed in the source. The diffusion time is 22h; the diffusion temperature is 1280±2℃; the diffusion junction depth is 40±5μm; the sheet resistance is 0.1Ω / □~0.3Ω / √.
[0095] 3. Grinding: Grind one side. The thickness of the silicon wafer after grinding is 250±10μm.
[0096] 4. Aluminum steaming: Aluminum is steamed on the retained phosphorus diffusion surface (fine grinding surface is not steamed), and the thickness of the aluminum layer is 13μm; after aluminum steaming, the alloy is alloyed, the alloy temperature is 500±10℃, and the constant temperature time is 5~10min.
[0097] 5. Splitting: Use ultrasonic cutting to split large pieces into Ф2 tube cores. The split chips are placed in HF:HNO3=1:5 (volume ratio) for corrosion, and the corrosion time is 80~110S; rinse with a large amount of cold deionized water and then dry.
[0098] 6. Mold assembly: Press the electrode lead, tube core, and aluminum sheet Figure 2 Assembled in a graphite mold. The diameter of the molybdenum electrode 3 is Φ2; the diameter of the copper lead 1 is Φ1.2, the composition of the aluminum sheet is silicon: aluminum = 5%, and the thickness of the aluminum sheet is 85μm.
[0099] 7. Alloy / welding: Vacuum degree: ≥3.4X10 -3 pa, temperature: 750~760℃, time: 30min~40min, naturally cool down to 450℃, the diode can be taken out below 100℃.
[0100] 8. Countertop corrosion: Place the diode in a KOH solution with a temperature of 92°C and a concentration of 8% for 5 minutes, take it out and rinse it with hot deionized water, boil it in hot deionized water for 5 times, and cross-rinse it with hot and cold deionized water for more than half an hour.
[0101] 9. Glass powder coating molding: The ratio of glass slurry is glass powder: water = 3g: 1ml. The product is completely coated with glass powder. High temperature molding: heat up to the maximum temperature of 650℃ for 20~70min, maintain for 1~3min, and the cooling rate is ≤3℃ / min.
Claims
1. A method for manufacturing a glass passivated solid package low voltage diode, characterized in that: The glass passivated solid package low-voltage diode comprises a silicon wafer A (5) and two electrode leads, wherein the silicon wafer A (5) is located between the two electrode leads, wherein one electrode lead is connected to the silicon wafer A (5) via a welding metal A (4), and the other electrode lead is connected to the silicon wafer A (5) via a welding metal B (7); the silicon wafer A (5), the welding metal A (4), the welding metal B (7) and the two electrode leads are all arranged in a passivation glass (6), and one end of the electrode lead extends outside the passivation glass (6); The silicon wafer A (5) is an N-type single crystal silicon wafer, comprising an N layer and an N+ layer, wherein the N layer is close to the welding metal A (4) and the N+ layer is close to the welding metal B (7); The electrode lead comprises a copper lead (1) and a molybdenum electrode (3), and the molybdenum electrode (3) is welded to the copper lead (1) via a silver-copper sheet (2); The welding metal A (4) is an aluminum sheet; The welding metal B (7) is a vaporized aluminum layer, and the vaporized aluminum layer has a thickness of 6 μm to 16 μm; The manufacturing method of the glass passivated solid package low-voltage diode comprises the following steps: Step 1, preparing a tube core; Step 2: high temperature sintering, welding the copper lead (1) and the molybdenum electrode (3) through the silver copper sheet (2) into a complete electrode lead; Step 3: vertically stack the electrode lead, the tube core, the aluminum sheet, and the electrode lead in the graphite mold in sequence, and then place the graphite mold in a vacuum sintering furnace to perform fusion welding bonding on the electrode lead, the tube core, and the aluminum sheet; Step 4: Insert the diode after welding into the corrosion tray, and use KOH solution with a concentration of 2-12% and a temperature of 80-100°C to corrode it for 3-7 minutes. After corrosion, rinse it with hot deionized water. After rinsing, put the diode into hot deionized water and boil it 3-7 times. Then take out the diode and cross-rinse it with hot and cold deionized water for more than half an hour. Step 5: Coat the surface of the diode with glass slurry, and then put it into a high-temperature molding furnace for molding; The tube core preparation in step 1 includes the following steps: A. Select N-type single crystal silicon wafer with a resistivity of 0.003Ω·cm ~0.04Ω·cm; B. Place N-type single crystal silicon wafer in the source for phosphorus diffusion to form N+NN+ silicon wafer, with a diffusion junction depth of 10μm ~80μm, a sheet resistance of 0.1Ω / □~3Ω / □, and a source ratio of P2O5:C2H5OH=5~6g:50ml; C. After phosphorus diffusion, the silicon wafer is subjected to grinding treatment to remove the N+ layer on one side, thereby forming an N N+ silicon wafer A (5). The thickness of the silicon wafer A (5) is 200 μm to 350 μm; D. Aluminum is evaporated on the N+ surface of the silicon wafer A (5), and the thickness of the aluminum vaporization layer is 6μm-16μm. After aluminum vaporization, the silicon wafer A (5) is placed in a vacuum sintering furnace, and the silicon wafer A (5) and the aluminum vaporization layer are fusion-bonded at a temperature of 450-550°C for 5-20 minutes. F. The silicon wafer A (5) is split into the required tube core size by ultrasonic cutting, and the chip obtained by the splitting is corroded by a solution with a volume ratio of HF:HNO3=1:5 for 80 to 180 seconds, and then the chip is rinsed with cold deionized water and dried to obtain the tube core; The core PN junction of the diode is obtained synchronously during the welding process of the electrode lead and the tube core. During high-temperature sintering, the N side of the tube core and the aluminum sheet alloy form the core PN junction of the diode. The obtained PN junction is a mutation junction, which can obtain a very low reverse voltage.
2. The method for manufacturing a glass passivated solid packaged low voltage diode according to claim 1, characterized in that: The aluminum sheet has a thickness of 40 μm to 100 μm, and a composition of silicon:aluminum = (0-15)%.
3. The method for manufacturing a glass passivated solid packaged low voltage diode according to claim 1, characterized in that: The vacuum degree in the vacuum sintering furnace in step 3 is ≥3.4×10 -3 pa, the fusion bonding temperature is 750~790℃, the fusion bonding time is 10min~60min, and the obtained diode is naturally cooled in a vacuum sintering furnace and taken out below 100℃.
4. The method for manufacturing a glass passivated solid packaged low voltage diode according to claim 1, characterized in that: In the step 5, the ratio of the glass powder slurry is glass powder: water = 3g: 1ml, the temperature in the high temperature molding furnace is increased to 650°C within 20-70 minutes, and then the temperature is lowered after being kept constant for 1-8 minutes, and the cooling rate is ≤3°C / min.